At Danchip we use as a standard a 28 wt% KOH.
At Danchip we use as a standard a 28 wt% KOH.
Wet etching of aluminium is done with two different solutions:
# H<math>_2</math>O:H<math>_3</math>PO<math>_4</math>  1:2 at 50 <sup>o</sup>C
# Pre-mixed etch solution: PES 77-19-04 at 20 <sup>o</sup>C
Both solutions are used in the Aluminium etch bath shown to the right. I must be written on which one is in. Solution no. 1 is the most used solution for etchning oure aluminium. Solution no. 2 is primarily for etching aluminium mixed with a small percentage of silicon.
<br clear="all" />
===Comparing the two solutions===
{| border="1" cellspacing="0" cellpadding="4" align="left"
!
! Aluminium Etch 1
! Aluminium Etch 2
|-
|General description
|
Etch of pure aluminium
|
Etch of aluminium + 1.5% Si
|-
|Chemical solution
|H<math>_2</math>O:H<math>_3</math>PO<math>_4</math>  1:2
|PES 77-19-04
|-
|Process temperature
|50 <sup>o</sup>C
|20 <sup>o</sup>C
|-
|Possible masking materials:
|
Photoresist (1.5 µm AZ5214E)
|
Photoresist (1.5 µm AZ5214E)
|-
|Etch rate
|
~100 nm/min (Pure Al)
|
~60(??) nm/min
|-
|Batch size
|
1-25 wafers at a time
|
1-25 wafer at a time
|-
|Size of substrate
|
4" wafers
|
4" wafers
|-
|Allowed materials
|
*Aluminium
*Silicon
*Silicon Oxide
*Silicon Nitride
*Silicon Oxynitride
*Photoresist
*E-beam resist
|
*Aluminium
*Silicon
*Silicon Oxide
*Silicon Nitride
*Silicon Oxynitride
*Photoresist