Specific Process Knowledge/Etch/Wet III-V Etches: Difference between revisions

From LabAdviser
Kabi (talk | contribs)
Bghe (talk | contribs)
No edit summary
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php?title=Specific_Process_Knowledge/Etch/Wet_III-V_Etches click here]'''  
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php?title=Specific_Process_Knowledge/Etch/Wet_III-V_Etches click here]'''  


This is a collection of III-V wet-etches; not all etches are currently used at DTU Danchip why the rates should be tested before use. Make sure you have the proper education in mixing of chemicals before use.
This is a collection of III-V wet-etches; the rates should be tested before use. Make sure you have the proper education in mixing of chemicals before use.


It is utterly important that your dispose of chemicals/etches according to the DTU Danchip regulations; more information is found in the III-V cleanroom.
It is utterly important that your dispose of chemicals/etches according to the DTU Danchip regulations; more information is found in the III-V cleanroom.
Line 9: Line 9:
==HCl:H3PO4 etch==
==HCl:H3PO4 etch==


HCl(37%):H<sub>3</sub>PO<sub>4</sub>(85%) is a selective, anisotropic and slow etching of InP. Very slow rate in quarternaries. The etch rates depend on the orientation of the features and have not yet been calibrated at DTU Danchip.
HCl(37%):H<sub>3</sub>PO<sub>4</sub>(85%) is a selective, anisotropic and slow etching of InP. Very slow rate in InGaAsP. The etch rates depend on the orientation of the features and have not yet been calibrated at DTU Danchip.


See rates below for InP, PQ(1.n) and InGaAs lattice-matched to InP. '''The acronym PQ(1.n) denotes a lattice-matched InGaAsP with a band gap corresponding to a wavelength of 1.n mm.'''  
See rates below for InP, PQ(1.n) and InGaAs lattice-matched to InP. '''The acronym PQ(1.n) denotes a lattice-matched InGaAsP on InP with a band gap corresponding to a wavelength of 1.n um.'''  


The temperature is 22 degC +/- 1 degC.
The temperature is 22 degC +/- 1 degC.


{| border="1" style="text-align: center; width: 400px; height: 100px;"
{| border="1" style="text-align: center; width: 600px; height: 100px;"
! colspan="4" style="text-align: center;" style="background: #efefef;" | HCl(37%):H<sub>3</sub>PO<sub>4</sub>(85%) etch rates, nm/min
! colspan="5" style="text-align: center;" style="background: #efefef;" | HCl(37%):H<sub>3</sub>PO<sub>4</sub>(85%) etch rates, nm/min
|-
|-
! scope="row" width="20%" |Etchant
! scope="row" width="20%" |Etchant
Line 22: Line 22:
! width="20%" |PQ(1.1)
! width="20%" |PQ(1.1)
! width="20%" |InGaAs
! width="20%" |InGaAs
! width="20%" |Contributer
|-
|-
|1:4
|1:4
Line 27: Line 28:
|<2
|<2
|<1
|<1
|Before 2012 by Tine Greibe
|-
|1:0
|8700 +/- 500
|&nbsp;
|small
|2014-July by Luisa Ottaviano
|}
|}


Line 33: Line 41:
==H2SO4:H2O2:H2O etch==
==H2SO4:H2O2:H2O etch==


H<sub>2</sub>SO<sub>4</sub>(10%):H<sub>2</sub>O<sub>2</sub>(35%):H<sub>2</sub>O is a selective etch of InGaAsP with very low etch rate in InP. '''The acronym PQ(1.n) denotes a lattice-matched InGaAsP with a band gap corresponding to a wavelength of 1.n mm.'''  
H<sub>2</sub>SO<sub>4</sub>(10%):H<sub>2</sub>O<sub>2</sub>(30%):H<sub>2</sub>O is a selective etch of InGaAsP with very low etch rate in InP. '''The acronym PQ(1.n) denotes a lattice-matched InGaAsP on InP with a band gap corresponding to a wavelength of 1.n um.'''  


The etchrates have not yet been calibrated at DTU Danchip.
The etchrates have not yet been calibrated at DTU Danchip.
The temperature is 22 degC +/- 1 degC.
The temperature is 22 degC +/- 1 degC.


{| border="1" style="text-align: center; width: 500px; height: 100px;"
{| border="1" style="text-align: center; width: 800px; height: 100px;"
! colspan="6" style="text-align: center;" style="background: #efefef;" | H<sub>2</sub>SO<sub>4</sub>(10%):H<sub>2</sub>O<sub>2</sub>(35%):H<sub>2</sub>O etch rates, nm/min
! colspan="7" style="text-align: center;" style="background: #efefef;" | H<sub>2</sub>SO<sub>4</sub>(10%):H<sub>2</sub>O<sub>2</sub>(30%):H<sub>2</sub>O etch rates, nm/min
|-
|-
! scope="row" width="20%" |Etchant
! scope="row" width="15%" |Etchant
! width="20%" |InP
! width="10%" |InP
! width="20%" |PQ(1.1)
! width="15%" |PQ(1.1)
! width="20%" |PQ(1.3)
! width="15%" |PQ(1.3)
! width="20%" |PQ(1.5)
! width="15%" |PQ(1.5)
! width="20%" |InGaAs
! width="15%" |InGaAs
! width="100%" |Contributer
|-
|-
|1:1
|1:1:0 '''<sup>1</sup>'''
|<5
|<5
|<50
|<50
|230+/-70
|1000+/-500
|2700+/-1000
|Updated 2014-July by Luisa Ottaviano
|-
|10:8:71
|&nbsp;
|&nbsp;
|&nbsp;
|&nbsp;
|500
|Updated 2014-July by Luisa Ottaviano
|-
|10:8:171
|&nbsp;
|&nbsp;
|&nbsp;
|&nbsp;
|&nbsp;
|&nbsp;
|&nbsp;
|180+/-20
|Updated 2014-July by Luisa Ottaviano
|}
|}


'''(1)''' The etchrates have not yet been calibrated at DTU Danchip.
<br>
<br>


==Concentrated H2SO4==
==Concentrated H2SO4==


Concentrated H<sub>2</sub>SO<sub>4</sub>(96%) is a selective etch of InP with a very low etch rate in InGaAsP.
Concentrated H<sub>2</sub>SO<sub>4</sub>(98%) is used for deoxidation of InP with a very low etch rate in InGaAsP.


{| border="1" style="text-align: center; width: 500px; height: 100px;"
{| border="1" style="text-align: center; width: 500px; height: 100px;"
! colspan="6" style="text-align: center;" style="background: #efefef;" | H<sub>3</sub>PO<sub>4</sub>(90%) etch rates, nm/min
! colspan="6" style="text-align: center;" style="background: #efefef;" | H<sub>2</sub>SO<sub>4</sub>(98%) etch rates, nm/min
|-
|-
! scope="row" width="20%" |Etchant
! scope="row" width="20%" |Etchant
Line 72: Line 99:
! width="20%" |InGaAs
! width="20%" |InGaAs
|-
|-
|H<sub>2</sub>SO<sub>4</sub>(96%)  
|H<sub>2</sub>SO<sub>4</sub>(98%)  
|13
|13
|?
|?
Line 84: Line 111:
==H3PO4:H2O2:H2O etch==
==H3PO4:H2O2:H2O etch==


H<sub>3</sub>PO<sub>4</sub>(85%):H<sub>2</sub>O<sub>2</sub>(35%):H<sub>2</sub>O is a GaAs/AlGaAs-etch which gives a better surface quality than H<sub>2</sub>SO<sub>4</sub>-based etches.
H<sub>3</sub>PO<sub>4</sub>(85%):H<sub>2</sub>O<sub>2</sub>(30%):H<sub>2</sub>O is a GaAs/AlGaAs-etch which gives a better surface quality than H<sub>2</sub>SO<sub>4</sub>-based etches.




{| border="1" style="text-align: center; width: 500px; height: 100px;"
{| border="1" style="text-align: center; width: 500px; height: 100px;"
! colspan="4" style="text-align: center;" style="background: #efefef;" | H<sub>3</sub>PO<sub>4</sub>(85%):H<sub>2</sub>O<sub>2</sub>(35%):H<sub>2</sub>O etch rates, nm/min
! colspan="4" style="text-align: center;" style="background: #efefef;" | H<sub>3</sub>PO<sub>4</sub>(85%):H<sub>2</sub>O<sub>2</sub>(30%):H<sub>2</sub>O etch rates, nm/min
|-
|-
! scope="row" width="30%" |Etchant
! scope="row" width="30%" |Etchant
Line 108: Line 135:
|~600
|~600
|~600
|~600
|'''2,3'''
|'''2, 3'''
|}
|}


'''(1)''' Temperature of mixture is ~22 C (no heating during etch). Data is obtained using magnetic stirring with sample on flat basket. '''(2)''' Refrigerated H2O used during mixture of etch, and mixture kept at 17 C during etch. '''(3)''' 10:2:30 gives smoother etch than 10:2:60.
'''(1)''' Temperature of mixture is ~22 degC (no heating during etch). Data is obtained using magnetic stirring with sample on flat basket. '''(2)''' Refrigerated H2O used during mixture of etch, and mixture kept at 17 degC during etch. '''(3)''' 10:2:30 gives smoother etch than 10:2:60.


<br>
<br>


==BHF etch==
==BHF, HF etch==


BHF etches SiO<sub>2</sub> and removes native oxide on InGaAs. '''Do not use BHF unless you know the dangers involved with this chemical and always use 4H gloves!'''.
BHF etches SiO<sub>2</sub> and partially removes native oxide on InGaAs and InP. '''Do not use BHF unless you know the dangers involved with this chemical and always use 4H gloves!'''.


{| border="1" style="text-align: center; width: 500px; height: 100px;"
{| border="1" style="text-align: center; width: 500px; height: 100px;"
! colspan="4" style="text-align: center;" style="background: #efefef;" | BHF etch rates, nm/min
! colspan="5" style="text-align: center;" style="background: #efefef;" | BHF (12.5%), HF etch rates, nm/min
|-
|-
! scope="row" width="30%" |Etchant
! scope="row" width="15%" |Etchant
! width="20%" |SiO<sub>2</sub> '''<sup>1</sup>'''
! width="25%" |SiO<sub>2</sub>
! width="20%" |PECVD2 Si<sub>3</sub>N<sub>4</sub>
! width="20%" |PECVD2 Si<sub>3</sub>N<sub>4</sub>
! width="20%" |E-beam Ti '''<sup>2</sup>'''
! width="20%" |E-beam Ti '''<sup>1</sup>'''
! width="20%" |Al(x)GaAs, x>0.5, AlAs
|-
|-
|BHF 1:7
|BHF (12.5%)
|202
|283 '''<sup>2</sup>''', 175+/-25 '''<sup>3</sup>'''
|52
|88 '''<sup>4</sup>'''
 
|90-120
|90-120
|&nbsp;
|-
|HF:H<sub>2</sub>O
|&nbsp;
|&nbsp;
|&nbsp;
|>10000 '''<sup>5</sup>'''
|}
|}


'''(1)''' Process '''SiO2thi1''' in PECVD2. '''(2)''' Ti from Titest.prg on Physimeca. It seems there is no measurable etchig during first 10 seconds.
'''(1)''' Ti from Titest.prg on Physimeca. It seems there is no measurable etchig during first 10 seconds.'''(2)''' Process '''SiO2ky2''' in PECVD2 (2014-July Luisa Ottaviamo @photonics ). '''(3)''' Process '''STANDARD''' in PECVD2 (2014-July Luisa Ottaviano @ photonics). '''(4)''' Process '''SINSTD''' in PECVD2 (2014-July Luisa Ottaviano @ photonics). '''(5)''' Appl. Phys. Lett. vol. 51, 2222 (1987).
 
<br>
<br>


Line 142: Line 175:
C<sub>6</sub>H<sub>8</sub>O<sub>7</sub>:H<sub>2</sub>O<sub>2</sub> is a selective etch of GaAs; does not etch Al<sub>x</sub>Ga<sub>{1-x}</sub>As if x > 0.45.
C<sub>6</sub>H<sub>8</sub>O<sub>7</sub>:H<sub>2</sub>O<sub>2</sub> is a selective etch of GaAs; does not etch Al<sub>x</sub>Ga<sub>{1-x}</sub>As if x > 0.45.


Solid C<sub>6</sub>H<sub>8</sub>O<sub>7</sub> is mixed 1:1 by weight with H<sub>2</sub>O using magnetic stirring. The solution C<sub>6</sub>H<sub>8</sub>O<sub>7</sub>:H<sub>2</sub>O is thereafter mixed 4:1 volume ratio with H<sub>2</sub>O<sub>2</sub>.
Solid C<sub>6</sub>H<sub>8</sub>O<sub>7</sub> is mixed 1:1 by weight with H<sub>2</sub>O (30%) using magnetic stirring. The solution C<sub>6</sub>H<sub>8</sub>O<sub>7</sub>:H<sub>2</sub>O is thereafter mixed 4:1 volume ratio with H<sub>2</sub>O<sub>2</sub>.


The above C<sub>6</sub>H<sub>8</sub>O<sub>7</sub>:H<sub>2</sub>O<sub>2</sub> solution has an etch-rate of ~360 nm/min in GaAs and < 0.5 nm/min in AlAs @ 25 C.
The above C<sub>6</sub>H<sub>8</sub>O<sub>7</sub>:H<sub>2</sub>O<sub>2</sub> solution has an etch-rate of ~360 nm/min in GaAs and < 0.5 nm/min in AlAs @ 25 degC.

Revision as of 09:16, 1 August 2014

Feedback to this page: click here

This is a collection of III-V wet-etches; the rates should be tested before use. Make sure you have the proper education in mixing of chemicals before use.

It is utterly important that your dispose of chemicals/etches according to the DTU Danchip regulations; more information is found in the III-V cleanroom.


HCl:H3PO4 etch

HCl(37%):H3PO4(85%) is a selective, anisotropic and slow etching of InP. Very slow rate in InGaAsP. The etch rates depend on the orientation of the features and have not yet been calibrated at DTU Danchip.

See rates below for InP, PQ(1.n) and InGaAs lattice-matched to InP. The acronym PQ(1.n) denotes a lattice-matched InGaAsP on InP with a band gap corresponding to a wavelength of 1.n um.

The temperature is 22 degC +/- 1 degC.

HCl(37%):H3PO4(85%) etch rates, nm/min
Etchant InP PQ(1.1) InGaAs Contributer
1:4 500 +/- 100 <2 <1 Before 2012 by Tine Greibe
1:0 8700 +/- 500   small 2014-July by Luisa Ottaviano


H2SO4:H2O2:H2O etch

H2SO4(10%):H2O2(30%):H2O is a selective etch of InGaAsP with very low etch rate in InP. The acronym PQ(1.n) denotes a lattice-matched InGaAsP on InP with a band gap corresponding to a wavelength of 1.n um.

The etchrates have not yet been calibrated at DTU Danchip. The temperature is 22 degC +/- 1 degC.

H2SO4(10%):H2O2(30%):H2O etch rates, nm/min
Etchant InP PQ(1.1) PQ(1.3) PQ(1.5) InGaAs Contributer
1:1:0 1 <5 <50 230+/-70 1000+/-500 2700+/-1000 Updated 2014-July by Luisa Ottaviano
10:8:71         500 Updated 2014-July by Luisa Ottaviano
10:8:171         180+/-20 Updated 2014-July by Luisa Ottaviano

(1) The etchrates have not yet been calibrated at DTU Danchip.

Concentrated H2SO4

Concentrated H2SO4(98%) is used for deoxidation of InP with a very low etch rate in InGaAsP.

H2SO4(98%) etch rates, nm/min
Etchant InP PQ(1.1) PQ(1.3) PQ(1.5) InGaAs
H2SO4(98%) 13 ? <1    


H3PO4:H2O2:H2O etch

H3PO4(85%):H2O2(30%):H2O is a GaAs/AlGaAs-etch which gives a better surface quality than H2SO4-based etches.


H3PO4(85%):H2O2(30%):H2O etch rates, nm/min
Etchant GaAs AlGaAs Comment
1:4:45 250 +/- 50 250 +/- 50 1
10:2:60 200 +/- 100 200 +/- 100 2
10:2:30 ~600 ~600 2, 3

(1) Temperature of mixture is ~22 degC (no heating during etch). Data is obtained using magnetic stirring with sample on flat basket. (2) Refrigerated H2O used during mixture of etch, and mixture kept at 17 degC during etch. (3) 10:2:30 gives smoother etch than 10:2:60.


BHF, HF etch

BHF etches SiO2 and partially removes native oxide on InGaAs and InP. Do not use BHF unless you know the dangers involved with this chemical and always use 4H gloves!.

BHF (12.5%), HF etch rates, nm/min
Etchant SiO2 PECVD2 Si3N4 E-beam Ti 1 Al(x)GaAs, x>0.5, AlAs
BHF (12.5%) 283 2, 175+/-25 3 88 4 90-120  
HF:H2O       >10000 5

(1) Ti from Titest.prg on Physimeca. It seems there is no measurable etchig during first 10 seconds.(2) Process SiO2ky2 in PECVD2 (2014-July Luisa Ottaviamo @photonics ). (3) Process STANDARD in PECVD2 (2014-July Luisa Ottaviano @ photonics). (4) Process SINSTD in PECVD2 (2014-July Luisa Ottaviano @ photonics). (5) Appl. Phys. Lett. vol. 51, 2222 (1987).

Citric Acid etch

C6H8O7:H2O2 is a selective etch of GaAs; does not etch AlxGa{1-x}As if x > 0.45.

Solid C6H8O7 is mixed 1:1 by weight with H2O (30%) using magnetic stirring. The solution C6H8O7:H2O is thereafter mixed 4:1 volume ratio with H2O2.

The above C6H8O7:H2O2 solution has an etch-rate of ~360 nm/min in GaAs and < 0.5 nm/min in AlAs @ 25 degC.