Specific Process Knowledge/Thin film deposition/Deposition of Silicon: Difference between revisions
Appearance
No edit summary |
No edit summary |
||
| Line 111: | Line 111: | ||
! Allowed material | ! Allowed material | ||
| | | | ||
* Silicon oxide | |||
* Silicon (oxy)nitride | |||
* Photoresist | |||
* PMMA | |||
* Mylar | |||
* SU-8 | |||
* Any metals | |||
| | | | ||
| | | | ||
Revision as of 14:06, 17 March 2014
Feedback to this page: click here
PolySilicon can be sputtered in Alcatel and be deposited in the PolySilicon furnace. In the chart below you can compare the two different deposition methodes:
| Sputter(PVD co-sputter/evaporation) | Furnace PolySi (Furnace LPCVD pSi) | Sputter (Wordentec) | Sputter (IBE/IBSD Ionfab 300) | Sputter (Alcatel) | |
|---|---|---|---|---|---|
| Batch size |
|
|
|
|
|
| Pre-clean | RF Ar clean | RCA clean for wafers that are not fresh form the box. | RF Ar clean | . | RF Ar clean |
| Layer thickness | 10Å to about 3000Å | ~50Å to 2µm, if thicker layers are needed please ask the furnace team. | 10Å to about 3000Å | . | 10Å to 2000Å |
| Deposition rate | Dependent on process parameters, but in the order of 1 Å/s. See more here |
|
.
Dependent on process parameters, but in the order of 1 Å/s. See more here. |
About 6-8 nm/min. See more here. | 2Å/s to 15Å/s |
| Process temperature | Option: heating wafer up to 400 deg C | 560 oC (amorph) and 620 oC (poly) | ? | . | ? |
| Step coverage | . | Good | . | . | Poor |
| Adhesion | . | Good for fused silica, silicon oxide, silicon nitride, silicon | . | . | Bad for pyrex, for other materials we do not know |
| Allowed substrates | Pyrex, fused silica, silicon, metals, oxide, nitride | Fused silica, Silicon, oxide, nitride | Pyrex, fused silica, silicon, metals, oxide, nitride | . |
|
| Allowed material |
|
| |||
| Doping facility | None | Can be doped during deposition with Boron and/or Phosphorous | None | . | None |
| Comment | This process is not running really stable nowadays. |
Sputtered Silicon in the Alcatel
| The parameter(s) changed | New value(s) | Deposition rate |
|---|---|---|
| Standard parameters | None | |
| Power | 400W | 3.8 Å/s |
Sputtered Silicon in the PVD co-sputter/evaporation
See this page: Si sputter in PVD co-sputter/evaporation
Sputtered Silicon in Wordentec
See this page: Si sputter in Wordentec