!Results  
!Results  
!Test on wafer with 20% load, by Izzet Yildiz @Nanotech
!Test on wafer with 20% load, ''by Izzet Yildiz @Nanotech''
|-
|-
|Etch rate of LPCVD nitride
|Etch rate of LPCVD nitride
|'''60-65 nm/min (20% etch load) (Feb.-2014)'''  
|'''60-65 nm/min (20% etch load) (Feb. 2014)'''  
|-
|-
|Selectivity to  resist [SiN : AZ resist]
|Selectivity to  resist [SiN : AZ resist]

Revision as of 14:23, 20 February 2014

Slow etch of silicon nitride with resist as masking material - with direct clamping

This recipe can be used for slow etching of silicon nitride with resist as masking material when normal clamping is possible. Normal clamping is prefered because it give the best and most repeatable cooling of the wafer. Here are some test results presented.

Parameter Resist mask
Coil Power [W] 200
Platen Power [W] 25
Platen temperature [oC] 0
CF4 flow [sccm] 20
H2 flow [sccm] 10
Pressure [mTorr] 3


Results Test on wafer with 20% load, by Izzet Yildiz @Nanotech
Etch rate of LPCVD nitride 60-65 nm/min (20% etch load) (Feb. 2014)
Selectivity to resist [SiN : AZ resist] 1:0.75
Wafer uniformity (100mm) ?
Profile [o] ?
Wafer uniformity map (click on the image to view a larger image) not measured
SEM profile images Not measured