Line 33: Line 33:
|-
|-
|Etch rate of thermal oxide
|Etch rate of thermal oxide
|'''64.9 nm/min (100% etch load) (22-01-2014)'''  
|'''44.1 nm/min (50% etch load) (01-02-2014)'''  
|-
|-
|Selectivity to  resist [:1]
|Selectivity to  resist [:1]
|No result
|~0.9
|-
|-
|Wafer uniformity (100mm)
|Wafer uniformity (100mm)
|'''±0.8% (22-01-2014)'''
|'''±1.6% (01-02-2014)'''
|-
|-
|Profile [<sup>o</sup>]
|Profile [<sup>o</sup>]
|Not tested
|Take a look at the iamges but be aware the the resist profile was not good to begin with.
|-
|-
|Images (click on the image to view a larger image)
|Images (click on the image to view a larger image)

Revision as of 09:44, 17 February 2014

Slow etch of SiO2 with resist as masking material - with direct clamping

This recipe can be used for slow etching of SiO2 with resist as masking material when normal clamping is possible. Normal clamping is prefered because it give the best and most repeatable cooling of the wafer. Here are some test results presented.

Parameter Resist mask
Coil Power [W] 200
Platen Power [W] 25
Platen temperature [oC] 0
CF4 flow [sccm] 20
H2 flow [sccm] 10
Pressure [mTorr] 3


Results Test on maskless wafer
Etch rate of thermal oxide 44.1 nm/min (50% etch load) (01-02-2014)
Selectivity to resist [:1] ~0.9
Wafer uniformity (100mm) ±1.6% (01-02-2014)
Profile [o] Take a look at the iamges but be aware the the resist profile was not good to begin with.
Images (click on the image to view a larger image)
Contour plot of the etch rate over the wafer, 9 points measured
Comments