Jump to content

Specific Process Knowledge/Back-end processing/Laser Micromachining Tool: Difference between revisions

From LabAdviser
Chasil (talk | contribs)
Chasil (talk | contribs)
Line 138: Line 138:
| Easily break silicon in cristal plan. Depth of the groove : 25µm  
| Easily break silicon in cristal plan. Depth of the groove : 25µm  
|- style="background:LightGray" valign="top"
|- style="background:LightGray" valign="top"
| Silicon 525µm with SiO2 (150nm to 1,2µm)
| Silicon 525µm with Si3N4 (150nm to 1,2µm)
| Red (1064nm/255mm)
| Red (1064nm/255mm)
| 200 kHz
| 200 kHz
Line 152: Line 152:
| Samples can easily be removed with a soft mecanical pressure. A layer of resist (AZMIR701) can be deposited on the top without influence the dicing. However, the burnt resist may induce cracks that can propagate, under the influence of the number of iteration. The blue tape may sticks to the wafer a the end of the process.   
| Samples can easily be removed with a soft mecanical pressure. A layer of resist (AZMIR701) can be deposited on the top without influence the dicing. However, the burnt resist may induce cracks that can propagate, under the influence of the number of iteration. The blue tape may sticks to the wafer a the end of the process.   
|-
|-
|- style="background:LightGray" valign="top"
| Ni (320µm)
| Green(532nm/255mm)
| 200 kHz
| 100%
| 0,64 W
| 300 mm/s
| 3 burst
| none
| 4320 it.
| 1
| N/A
| [[media:Cutting_Ni_320µm.xls|Cutting Ni 320µm]]
| Cutting through only blue tape left
|-
|- style="background:LightGray" valign="top"
| Pyrex 1000µm
| Red(1064nm/255mm)
| 200 kHz
| 100%
| 2,8 W
| 1000 mm/s
| 1 burst
| none
| 99 it.
| 13 
| 20 µm
| [[media:Cutting_Pyrex_microfluidic_hole_1064nm_255mm.xls|Cutting Pyrex 1000µm for microfluidic hole parameters]]
| Increase/decrease the number of iteration to increase/decrease the width of the hole. [[file:pyrex_10um_hole_chanel.jpg|Microscope view of the chanel  ]]
|-
|}
|}



Revision as of 17:05, 7 January 2014

Feedback to this page: click here

Laser Micromachining Tool

Lasertool microSTRUCT vario (3D-Micromac AG)
Inside lasertool

The Laser Micromachining Tool is a microSTRUCT vario from the company 3D-Micromac AG.

The system is able to produce micro structures in different kinds of materials like metals, ceramics, composite materials, etc.

The machine is located in the basement of building 346 under the cleanroom.

The user manual(s), user APV(s), technical information and contact information can be found in LabManager:

The Laser Micromachining Tool in LabManager

It is equipped with 2 high power lasers:

  • a 50W picosecond laser that can emit light at 3 wavelengths: 355nm, 532nm and 1064nm and a
  • a 100W nanosecond laser with a wavelength of 1064nm.

It consist of these main parts:

  • Upper service way
  • Manual front door
  • Operating panel
  • Machine's feet (adjustable)
  • Left service way
  • Electrical cabinet

Process information

Laser Processing details

Material Pattern Optics Frequency Intensity Writing speed Other Parameter file
Silicon Red (1064nm/255mm) 100% ?? mm/s silicon cutting.par
Silicon with SiliconNitride Red (1064nm/255mm) 100% ?? mm/s silicon-SiN cutting.par
Borofloat glass Red (1064nm/255mm) 100% ?? mm/s borofloat cutting.par
Nickel Red (1064nm/255mm) 100% ?? mm/s nickel cutting red.par
Nickel "wafer" 85mm diameter Green (532nm/255mm) 200 kHz 100% 300 mm/s Fixed Burst mode, 3 pulses. Sky writing mode 3. nickel cutting green parameters
Mask making Blue (355nm/103mm) 20% ?? mm/s mask making.par


Material Optics Frequency Intensity Power measured @10% Writing speed Number of burst Number of Z-offset Number of iteration Number of parallel lines Gap in between line Parameter file Comments
Silicon 525µm Green(532nm/255mm) 200 kHz 100% 0,57 W 50 mm/s 1 burst none 4 it. 1 N/A Silicon dicing green parameters Easily break silicon in cristal plan. Depth of the groove : 25µm
Silicon 525µm with Si3N4 (150nm to 1,2µm) Red (1064nm/255mm) 200 kHz 100% 2,8 W 1000 mm/s 3 bursts 1 (-0,3mm) 350/100 4 50 µm Silicon nitride cutting parameters Samples can easily be removed with a soft mecanical pressure. A layer of resist (AZMIR701) can be deposited on the top without influence the dicing. However, the burnt resist may induce cracks that can propagate, under the influence of the number of iteration. The blue tape may sticks to the wafer a the end of the process.
Ni (320µm) Green(532nm/255mm) 200 kHz 100% 0,64 W 300 mm/s 3 burst none 4320 it. 1 N/A Cutting Ni 320µm Cutting through only blue tape left
Pyrex 1000µm Red(1064nm/255mm) 200 kHz 100% 2,8 W 1000 mm/s 1 burst none 99 it. 13 20 µm Cutting Pyrex 1000µm for microfluidic hole parameters Increase/decrease the number of iteration to increase/decrease the width of the hole. Microscope view of the chanel



The parameter filename extension is here set to .doc because of MediaWiki restrictions. The 3DMM laser software uses .par as parameter file extension.
The file should be a pure text-file with no formatting codes etc.