The SOI etch uses the Low frequency (LF) platen generator to minimize the notching at buried stop layers such as the BOX layer in a SOI wafer. | The SOI etch uses the Low frequency (LF) platen generator to minimize the notching at buried stop layers such as the BOX layer in a SOI wafer. | ||
{| class="wikitable collapsible autocollapse" | |||
! Simple collapsible table | |||
|- | |||
| Lorem ipsum dolor sit amet | |||
|} | |||
{| border="2" cellpadding="2" cellspacing="1" style="text-align:center;" | {| border="2" cellpadding="2" cellspacing="1" style="text-align:center;" | ||
Revision as of 13:57, 30 April 2014
Feedback to this page: click here
SOI etch
The SOI etch uses the Low frequency (LF) platen generator to minimize the notching at buried stop layers such as the BOX layer in a SOI wafer.
| Simple collapsible table |
|---|
| Lorem ipsum dolor sit amet |
| Parameter | Specification | Average result |
|---|---|---|
| Etch rate (µm/min) | > 10 | 10.7 |
| Etched depth (µm) | 100 | 107 |
| Scallop size (nm) | < 800 | 685 |
| Profile (degs) | 91 +/- 1 | 90.7 |
| Selectivity to AZ photoresist | > 100 | 183 |
| Undercut (µm) | <1.5 | 0.89 |
| Uniformity (%) | < 3.5 | 2.7 |
| Repeatability (%) | <4 | 0.47 |
| Main etch (D->E) | Etch | Dep |
|---|---|---|
| Gas flow (sccm) | SF6 400 O2 40 | C4F8 250 |
| Cycle time (secs) | 3.0 | 2.0 |
| Pressure (mtorr) | 30 | 25 |
| Coil power (W) | 2800 | 2000 |
| LF Platen power (W) | 75 | 0 |
| LF Platen Pulsing software set-up | 0.025s, 75% | - |
| Cycles | 96 (process time 08:00) | |
| Common | Temperature 20 degs, HBC 10 torr, Long funnel, with baffle & 100 mm spacers | |