Specific Process Knowledge/Etch/Wet Gold Etch: Difference between revisions
Appearance
No edit summary |
No edit summary |
||
| Line 4: | Line 4: | ||
==Etching of Gold== | ==Etching of Gold== | ||
[[Image:fumehoodetch-gold.jpg |300x300px|thumb|Wet Gold Etch: Done in the fumehood positioned in cleanroom 2]] | [[Image:fumehoodetch-gold.jpg |300x300px|thumb|Wet Gold Etch: Done in the fumehood positioned in cleanroom 2]] | ||
Etching of Gold is done wet at Danchip making your own set up in a beaker in the fumehood. You can see the APV [http:// | Etching of Gold is done wet at Danchip making your own set up in a beaker in the fumehood. You can see the APV [http://labmanager.danchip.dtu.dk/d4Show.php?id=2479&mach=146 here]. | ||
We have two different solutions: | We have two different solutions: | ||
Revision as of 15:35, 4 September 2013
Ething of Gold can be done either wet or dry. For wet etching please see below on this page. Dry etching can be done with IBE by sputtering with Ar ions.
Etching of Gold

Etching of Gold is done wet at Danchip making your own set up in a beaker in the fumehood. You can see the APV here.
We have two different solutions:
- Iodine etch: KI:I2:H2O - 100g:25g:500ml - standard at Danchip. Can be used with AZ resist as mask.
- Aqua Regia (Kongevand): HNO3:HCl - 1:3 - A very strong acid witch will etch most metals and are therefore used when you wish to remove all the gold from your wafer. you have to be very carefull when you work with Aqua Regia (Kongevand) It can generate nitrous gases witch are very toxic!!
Comparing the two solutions
| Iodine based gold etch | Aqua Regia (Kongevand) | |
|---|---|---|
| General description |
Etch of pure Gold with or without photoresist mask. |
Etch of pure Gold (as stripper). |
| Link to safety APV | see APV here. | see APV here |
| Chemical solution | KI:I2:H2O (100g:25g:500ml) | HCl:HNO3 (3:1) |
| Process temperature | 20 oC | 20 oC |
| Possible masking materials |
Photoresist (1.5 µm AZ5214E) |
Unmasked - used as a stripper |
| Etch rate |
~100 nm/min |
~(??) nm/min - fast etch |
| Batch size |
1-5 4" wafers at a time |
1-5 4" wafer at a time |
| Size of substrate |
2-6" wafers |
2-6" wafers |