The process runs for 31 cycles (5:56 mins). The fact that it's Bosch process is clear from the scallops on the sidewalls - one should be able to count 31 of them.  
The process runs for 31 cycles (5:56 mins). The fact that it's Bosch process is clear from the scallops on the sidewalls - one should be able to count 31 of them.  
The process is designed to reach 20 <math>\mu</math>m down in a 2 <math>\mu</math>m trench but as is clear from the image of the corresponding 50 <math>\mu</math>m trench, this one is etched deeper.
The process is designed to reach 20 <math>\mu</math>m down in a 2 <math>\mu</math>m trench but as is clear from the image of the corresponding 50 <math>\mu</math>m trench, this one is etched deeper.
<gallery caption="Sample gallery" widths="300px" heights="300px" perrow="2">
[[Image:jmlshal070921 pos1 2mu_09.jpg|Standardization image of the profile of a 2 <math>\mu</math>m trench created by the shallolr recipe]]
[[image:jmlshal070921 pos1 50mu_08.jpg|Standardization image of the profile of a 50 <math>\mu</math>m trench created by the shallolr recipe]]
</gallery>


[[image:jmlshal070921 pos1 2mu_09.jpg|370x370px|thumb|left|Standardization image of the profile of a 2 <math>\mu</math>m trench created by the shallolr recipe]]
[[image:jmlshal070921 pos1 2mu_09.jpg|370x370px|thumb|left|Standardization image of the profile of a 2 <math>\mu</math>m trench created by the shallolr recipe]]

Revision as of 16:02, 11 December 2007

The ASE

The ICP-DRIE (Inductively Coupled Plasma - Deep Reactive Ion Etcher) tool at Danchip is manufactured by STS and is called the ASE (Advanced Silicon Etcher). The main purpose of the ASE is etching of silicon using Bosch process.

The Bosch process: Etching of silicon

The Bosch process uses alternation between an etch cycle and a passivation cycle. Introducing a passivation step in an etch process is very beneficial for the control of the angle of the sidewalls in the etch process because it allows us to cover them with a protective layer that suppresses the isotropic etching. Combined with the high plasma density in the ICP chamber, the excellent sidewall control enables us to etch high aspect ratio structures in silicon with very high etch rates.

In the case of the silicon etching on the ASE, an etch phase with SF6 and O2 alternates with a passivation phase with C4F8.

The two standard silicon etch recipes

Two recipes have been optimized for the ASE. Their specification is on a 10 % etch load wafer with trenches.

  • Shallolr: The shallow etch process will etch a 2 μm opening down to make a 20 μm trench.
  • Deepetch: The deep etch process will etch a 50 μm opening down to make a 300 μm trench.

The standardization procedure on the ASE covers these two etches.

Recipes on the ASE

Shallolr

The shallolr recipe is designed to etch features (with sizes above 1 μm) in silicon down to a depth that ranges from a few microns to some 50 microns. If you need to etch deeper use Deepetch or more shallow, see Nanoetches.

The recipe is given below.

The shallolr recipe
Common parameters Multiplexed parameters
Parameter Setting Parameter Etch Passivation
Temperature 10oC SF6 Flow 260 sccm 0 sccm
No. of cycles 31 O2 Flow 26 sccm 0 sccm
Process time 5:56 mins C4F4 Flow 0 sccm 120 sccm
APC mode manual RF coil 2800 W 1000 W
APC setting 86.8 % RF Platen 16 W 0 W
Cycle time 6.5 s 5 s

The process runs for 31 cycles (5:56 mins). The fact that it's Bosch process is clear from the scallops on the sidewalls - one should be able to count 31 of them. The process is designed to reach 20 μm down in a 2 μm trench but as is clear from the image of the corresponding 50 μm trench, this one is etched deeper.

Standardization image of the profile of a 2 μm trench created by the shallolr recipe
Standardization image of the profile of a 50 μm trench created by the shallolr recipe







Deepetch

The deepetch recipe
Common parameters Multiplexed parameters
Parameter Setting Parameter Etch Passivation
Temperature 20oC SF6 Flow 230 sccm 0 sccm
No. of cycles 250 O2 Flow 23 sccm 0 sccm
Process time 54:10 mins C4F4 Flow 0 sccm 120 sccm
APC mode manual RF coil 2800 W 1000 W
APC setting 87.7 % RF Platen 19 W 0 W
Cycle time 8 s 5 s


Standardization procedure on the ASE