At the moment DANCHIP has 3 PECVDs that can deposite silicon nitride and silicon oxynitride. PECVD1 and PECVD3 are for silicon based processing. PECVD2 is for III-V processing and will be describes under III-V processing. Look at the [[Specific Process Knowledge/Thin film deposition/PECVD|PECVD]] page to learn more about the PECVDs at DANCHIP. All though PECVD1 and PECVD3 are very much alike you cannot count on the a recipe on one system will give exactly the same results on the other system.
At the moment DANCHIP has 3 PECVDs that can deposite silicon nitride and silicon oxynitride. PECVD1 and PECVD3 are for silicon based processing. PECVD2 is for III-V processing and will be describes under III-V processing. Look at the [[Specific Process Knowledge/Thin film deposition/PECVD|PECVD]] page to learn more about the PECVDs at DANCHIP. All though PECVD1 and PECVD3 are very much alike you cannot count on the a recipe on one system will give exactly the same results on the other system.
== Deposition of SiN with PECVD4 [[Image:section under construction.jpg|70px]] ==
{| border="1" cellspacing="2" cellpadding="2"
|-style="background:Black; color:White"
! Parameter
|Recipe name: '''SiO2_res''' ('''SiO2''' etch with '''res'''ist mask) 
|-
|Coil Power [W]
|1300
|-
|Platen Power [W]
|200
|-
|Platen temperature [<sup>o</sup>C]
|0
|-
|He flow [sccm]
|174
|-
|C<sub>4</sub>F<sub>8</sub> flow [sccm]
|5
|-
|H<sub>2</sub> flow [sccm]
|4
|-
|Pressure [mTorr]
|4
|-
|}
{| border="2" cellspacing="2" cellpadding="3"
|-style="background:DarkGray; color:White"
!Material to be etched
!Etch rate using SiO2_res
|-
|Thermal oxide
|
*'''~230nm/min (5% etch load)''' -  etch load dependency [[/AOE SiO2 etch load dependency|'''see here''']]
*~200 nm/min ''fall 2016 by Martin Lind Ommen @nanotech''
|-
|TEOS oxide (5% load)
|'''233nm/min &plusmn;0.7%''' - "&plusmn;" represents the non-uniformity over a 100mm wafer - etched in Marts 2013 ''by LN/BGE@danchip''
|-
|PECVD1 (standard) oxide (5% load)
|'''242nm/min &plusmn;0.6%''' - "&plusmn;" represents the non-uniformity over a 100mm wafer - etched in Marts 2013 by ''LN/BGE@danchip''
|-
|Al2O3 from the ALD
|
*34.2 nm/min (1:6 to SiO2) ''fall 2016 by Martin Lind Ommen @nanotech''
*50nm can be etched in 10min - [[/Etch of Al2O3|'''See results here''']] etched in November 2014 by ''FRSTO@danchip''
|-
|Silicon rich nitride from furnace B2
|136nm was etched in 1min (whole wafer) - etched in October 2015 by ''bghe@danchip''
|-
|Cr
|6 nm/min (1:33 to SiO2) ''fall 2016 by Martin Lind Ommen @nanotech''
|-
|Al
|25nm/min (1:8 to SiO2) ''fall 2016 by Martin Lind Ommen @nanotech''
|-
|}
<br clear="all" />


==Recipes on PECVD2 for deposition of silicon nitride and silicon oxynitride ==