Jump to content

Specific Process Knowledge/Etch/Wet Silicon Oxide Etch (BHF): Difference between revisions

From LabAdviser
Kb (talk | contribs)
Hvje (talk | contribs)
 
(150 intermediate revisions by 11 users not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:Wetchemistry@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Etch/Wet_Silicon_Oxide_Etch_(BHF) click here]'''
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/Wet_Silicon_Oxide_Etch_(BHF) click here]'''


'''''Unless anything else is stated, everything on this page, text and pictures are made by DTU Nanolab.'''''


==Wet Silicon Oxide Etch (BHF and SIO Etch (wetting agent))==
'''''All links to Kemibrug (SDS) and Labmanager Including APV, requires login.'''''
[[Image:BHF_RR3.jpg|300x300px|thumb|Wet Silicon Oxide Etch (BHF): positioned in cleanroom 3]]
[[Image:BHF_wetting.jpg|300x300px|thumb|SIO etch (BHF with wetting agent): positioned in cleanroom 4]]
[[Image:KOH_4tommer.jpg|225x225px|thumb|BHF between the KOH baths: positioned in cleanroom 3. This is primarily used to remove oxide before and after a KOH etch]]
[[Image:Fumehoodetch-chrom2.jpg|225x225px|thumb|PP-bath: positioned in fume hood in cleanromm 2]]


[[index.php?title=Category:Equipment|Etch Wet Silicon Oxide]]
[[index.php?title=Category:Etch (Wet) bath|Silicon Oxide]]


Silicon oxide can be etched using HF. At Danchip it is mainly used in a buffered version BHF (premixed). The BHF has a more stable etch rate and is more gentle to photoresist due to an almost pH neutral solution which makes photoresist a good masking material for the oxide etch.
==Wet Silicon Oxide Etch (BHF, HF and BOE 7:1 Etchant VLSI)==


SIO etch (BHF with wetting agent) can also be used for etching silicon oxide. This is mainly for etching small holes. If you have wetting problems in BHF try the SIO etch. It is also a good idea to wet the sample in water for a few minutes before etching.
Silicon oxide can be etched using HF. At DTU Nanolab it is mainly used in a buffered version BHF (premixed). You can find safety datasheets on Kemibrug [http://kemibrug.dk here] The BHF has a stable etch rate and is gentle to photoresist due to an almost pH neutral solution which makes photoresist a good masking material for the oxide etch.  


Wafers with metals or other materials, not allowed in the dedicated oxide etch baths, can be etched in the PP-bath positioned in the fume hood in cleanroom 2 or in a '''plastic''' beaker.  
BOE 7:1 Etchant VLSI with Surfactant (BHF with wetting agent) can also be used for etching silicon oxide. This is mainly for etching small holes. At DTU Nanolab we do not have BHF with wetting agent in a prepared bath, it's only to be used in fumehoods. It's not very often used and we do not have it as a standard chemical. Please contact DTU Nanolab if you need it.


===Silicon oxide etch data===
Wafers with metals or other materials, not allowed in the dedicated oxide etch baths, can be etched using a '''plastic beaker''' in Fume hood 01 or 02 (Acids/bases) in D-3. Samples with III-V materials (e.g. InP and GaAs) must be etched in Fume hood 07: III-V Avids/bases in D-3.
{| border="2" cellspacing="0" align="left" cellpadding="5"
<br>
!
 
! BHF
'''The user manual for Oxide etch 1: BHF, APV's and contact information can be found in LabManager''' [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=389 by clicking here]
! 5% HF
 
! 40 % HF
'''The user manual for Oxide etch 2: BHF (clean), APV's and contact information can be found in LabManager''' [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=378 by clicking here]
! SIO
 
|-valign="top"
'''The user manual for Oxide etch 3: 10% HF, APV's and contact information can be found in LabManager''' [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=380 by clicking here]
|'''General description'''
 
|
'''The user manual for various HF baths in RCA and Fume hoods, APV's and contact information can be found in LabManager''' [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=64 by clicking here]
Etching of silicon oxide with a stable etch rate
 
|
'''<big>Working with HF above 13% is only allowed by Nanolab staff</big>'''
Mainly for removing native oxide
 
|
<!-- remember to remove the type of documents that are not present -->
Mainly for etching deep into borofloat or quartz wafers
 
|
 
Etching of silicon oxide - especially for etching small holes
'''Process information:''' <br>
|-valign="top"
See more [[/BHF etch rates|etch rates]] in HF solutions.
|'''Link to safety APV and KBA'''
 
|[http://www.labmanager.danchip.dtu.dk/d4Show.php?id=1897&mach=64 see APV here]
 
[http://kemibrug.dk/KBA/CAS/106534/?show_KBA=1&portaldesign=1 see KBA here]
{| border="2" cellspacing="0" cellpadding="2"
|[http://www.labmanager.danchip.dtu.dk/d4Show.php?id=1897&mach=64 see APV here]
[http://kemibrug.dk/KBA/CAS/106534/?show_KBA=1&portaldesign=1 see KBA here]
|[http://www.labmanager.danchip.dtu.dk/d4Show.php?id=2479&mach=146 see APV here]
[http://kemibrug.dk/KBA/CAS/100648/?lang=da&show_KBA=1&portaldesign=1 see KBA here]
|[http://www.labmanager.danchip.dtu.dk/d4Show.php?id=1897&mach=64 see APV here]
[ see KBA here]


|-valign="top"
!colspan="2" border="none" style="background:silver; color:black;" align="center"|Etchant
|'''Chemical solution'''
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Etch/Wet_Silicon_Oxide_Etch_(BHF)#Comparing_different_BHF_baths|BHF]]</b>
|BHF
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Etch/Wet_Silicon_Oxide_Etch_(BHF)#Comparing_different_5.25_HF_baths|1% HF / 5% HF / 10% HF]]</b>
|5% HF
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Etch/Wet_Silicon_Oxide_Etch_(BHF)#Comparing_different_40.25_HF_baths|40% HF]]</b>
|40% HF
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Etch/Wet_Silicon_Oxide_Etch_(BHF)#SiO_etch_bath|BOE 7:1 Etchant VLSI with Surfactant]]</b>
|BHF with wetting agent
|-
|-valign="top"
!style="background:silver; color:black;" align="center" width="60" rowspan="2"|Purpose
|'''Process temperature'''
|style="background:LightGrey; color:black"|Etching of silicon oxide 
|Room temperature
|style="background:WhiteSmoke; color:black"|
|Room temperature
*Etching of silicon oxide with a stable etch rate
|Room temperature
|style="background:WhiteSmoke; color:black"|
|Room temperature
*Mainly for removing native oxide
|-valign="top"
|style="background:WhiteSmoke; color:black"|
|'''Possible masking materials'''
*Mainly for etching deep into borofloat or quartz wafers. '''Only Nanolab staff are allowed to work with this HF'''.
|
|style="background:WhiteSmoke; color:black"|
*Etching of silicon oxide - especially for etching small holes
|-
|style="background:LightGrey; color:black"|Link to safety APV and SDS (You must be logged in to Kemibrug to view SDSs)
|style="background:WhiteSmoke; color:black"|
*:[http://labmanager.nanolab.dtu.dk/d4Show.php?id=1897&mach=64 see APV here]
*:[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhESkhKSUxMVGQlYzIlODclN2N2JWMyJTgzJTdlJWMyJTg4diVjMiU4OSU3ZSVjMiU4NCVjMiU4MyVjMiU4OCU1ZVlSSQ==#K see SDS here]
|style="background:WhiteSmoke; color:black"|
*:[http://labmanager.danchip.dtu.dk/d4Show.php?id=1897&mach=64 see APV here]
*:[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhERkZMSkhFR1RkJWMyJTg3JTdjdiVjMiU4MyU3ZSVjMiU4OHYlYzIlODklN2UlYzIlODQlYzIlODMlYzIlODglNWVZUkk=#K see SDS here]
|style="background:WhiteSmoke; color:black"|
*:[http://labmanager.danchip.dtu.dk/d4Show.php?id=2479&mach=146 see APV here]
*:[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhERkZMSkhOSVRkJWMyJTg3JTdjdiVjMiU4MyU3ZSVjMiU4OHYlYzIlODklN2UlYzIlODQlYzIlODMlYzIlODglNWVZUkk=#K see SDS here]
|style="background:WhiteSmoke; color:black"|
*:[http://labmanager.danchip.dtu.dk/d4Show.php?id=1897&mach=64 see APV here]
*:[https://kemibrug.dk/Kemikalier/Action?id=RCU2MHolYzIlODIlN2UlYzIlODB2JWMyJTgxJTdleiVjMiU4N0RZeiVjMiU4OXYlN2UlYzIlODElYzIlODhERkVKS0lNTFRkJWMyJTg3JTdjdiVjMiU4MyU3ZSVjMiU4OHYlYzIlODklN2UlYzIlODQlYzIlODMlYzIlODglNWVZUkk=#K see SDS here]
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Performance
|style="background:LightGrey; color:black"|Isotropic
|style="background:WhiteSmoke; color:black"|
*Isotropic
|style="background:WhiteSmoke; color:black"|
*Isotropic
|style="background:WhiteSmoke; color:black"|
*Isotropic
|style="background:WhiteSmoke; color:black"|
*Isotropic
|-
|style="background:LightGrey; color:black"|Etch rates
[[/BHF etch rates|See more]]
|style="background:WhiteSmoke; color:black"|
*Wet thermal oxide:75-80nm/min
|style="background:WhiteSmoke; color:black"|
*Wet thermal oxide:~6nm/min(1%) / 25nm/min(5%) / 52nm/min(10%)
|style="background:WhiteSmoke; color:black"|
*Boronfloat and quartz: ~3-4 μm/min
|style="background:WhiteSmoke; color:black"|
*Thermal oxide 80 nm/min
|-
|style="background:LightGrey; color:black"|Lifetime of photoresist
|style="background:WhiteSmoke; color:black"|
*~½ hour
|style="background:WhiteSmoke; color:black"|
*~½ hour
|style="background:WhiteSmoke; color:black"|
*~½ hour
|style="background:WhiteSmoke; color:black"|
*~½ hour
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Process parameter range
|style="background:LightGrey; color:black"|Chemical solution
|style="background:WhiteSmoke; color:black"|
*BHF (12%HF with Ammoniumflouride)
|style="background:WhiteSmoke; color:black"|
*1% / 5% HF
|style="background:WhiteSmoke; color:black"|
*40% HF
|style="background:WhiteSmoke; color:black"|
*BOE 7:1 Etchant VLSI with Surfactant (BHF with a wetting agent)
|-
|style="background:LightGrey; color:black"|Temperature
|style="background:WhiteSmoke; color:black"|
*Room temperature
|style="background:WhiteSmoke; color:black"|
*Room temperature
|style="background:WhiteSmoke; color:black"|
*Room temperature
|style="background:WhiteSmoke; color:black"|
*Room temperature
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="1"|Substrates
|style="background:LightGrey; color:black"|Masking material
|style="background:WhiteSmoke; color:black"|
*Silicon nitride
*Poly silicon
*Photoresist
*Photoresist
*Blue film
|style="background:WhiteSmoke; color:black"|
*Silicon nitride
*Silicon nitride
*PolySi
*Poly silicon
*Photoresist delaminates
*Blue film
*Blue film
 
|style="background:WhiteSmoke; color:black"|
In RCA bench:
*Photoresist delaminates
*No masking material
*Silicon nitride (Only on quartz wafers)
|
*Poly silicon (Only on quartz wafers)
In '''plastic''' beaker or PP-bath in the fume hood in cleanroom 2:
*Blue film
*Chromium and gold
|style="background:WhiteSmoke; color:black"|
*Silicon nitride
*Poly silicon
*Photoresist
*Photoresist
*Silicon nitride
*PolySi
*Blue film
*Blue film
|-
|}
==Life time of the photoresist and blue film in BHF==
Photoresist delaminates from the substrate in BHF. For standard photoresist this process starts after about or less than ½ hour but the time can vary with resist pattern. It starts by under etching the photoresist at the edges. The life time can be prolonged a little to ½ hour - 40 minutes if the photoresist is baked at 120<sup>o</sup>C.
Blue film also has a limited life time in BHF. Blue film is mainly used for back side protecting the wafer while etching on the front side. The life time of Blue film is also about ½ hour.


In RCA bench:  
<br clear="all" />
*No masking material
 
<gallery caption="Different places to do wet silicon oxide etch" widths="420px" heights="425px" perrow="5"> image:BHF clean.JPG|BHF in wetbench 04 in D-3 (Oxide etch 2: BHF (clean)). Wet silicon oxide etch bath positioned to the right in the wetbench. This bath can also be used for BHF with wetting agent.
image:KOH_BHF.JPG|BHF in wetbench 01 Si etch in D-3 (Oxide etch 1: BHF). The BHF bath is positioned in the middle of the bench. This is primarily used to remove oxide before and after a Si etch.
image:BHF clean.JPG|BHF in wetbench 05 in D-3 (Oxide etch 3: 10% HF). Wet silicon oxide etch bath positioned to the right in the wetbench. This bath can also be used for BHF, BHF with wetting agent or 40% HF on request. This bath is also used for cleaning quarts carriers from the PECVD4 system.
image:RCA-HF.jpg|HF baths in RCA bench in B-1. These may only be used together with RCA cleaning and furnace processes.
</gallery>
 
 
<br clear="all" />
 
==Comparing different BHF baths==
{|border="1" cellspacing="1" cellpadding="3" style="text-align:left;"
|-
 
|-style="background:silver; color:black"
!
! BHF (KOH) in D-3(Oxide etch 1: BHF)
! BHF clean in D-3 (Oxide etch 2: BHF)
! BHF in RCA Bench
! BHF in PP-bath
! BHF Plastic beaker
 
|-
|-style="background:WhiteSmoke; color:black"
!Batch size!
|1-25 wafers at a time
|1-25 wafer at a time
|1-25 wafers at a time
|1-25 wafers at a time
|1-7 wafers at a time
|-
 
|-style="background:LightGrey; color:black"
!Size of substrate
|2"-6" wafers
|2"-6" wafers
|2"-6" wafers
|2"- 4" wafers or any that fits in a dedicated holder
|2"- 4" wafers or any that fits in a dedicated holder
|-
 
|-style="background:WhiteSmoke; color:black"
!Allowed materials
|
|
In '''plastic''' beaker with magnetic stirrer in the fume hood in cleanroom 2:
*Silicon
*Poly Silicon
*Silicon Oxide
*Silicon Nitride
*Silicon Oxynitride
*Photoresist
*Photoresist
*Silicon nitride (Only on quartz wafers)
*PolySi(Only on quartz wafers)
*Blue film
*Blue film
*Chromium and gold
|
|
*Silicon
*Poly Silicon
*Silicon Oxide
*Silicon Nitride
*Silicon Oxynitride
*Photoresist
*Photoresist
*Silicon nitride
*PolySi
*Blue film
*Blue film
|-valign="top"
|'''Etch rate'''
|
*Wet thermal oxide:~80nm/min
*PECVD1 (standard):~147nm/min
*TEOS:~265nm/min
*Stoichiometric Si3N4:~0.75nm/min (Morten Bo Mikkelsen, March 2013)
|
*Wet thermal oxide:~25nm/min
*PECVD1 (standard):~87nm/min
*TEOS:~153nm/min
|
*Boronfloat and quartz: ~3-4 &mu;m/min
|
A little higher etch rates than BHF
|-valign="top"
|'''[[#Life_time_of_the_photoresist_and_blue_film_in_BHF|Life time of the photoresist]]'''
|~½ hour
|~½ hour
|~½ hour
|~½ hour
|-valign="top"
|'''Batch size'''
|
Plastic beaker:
*1-5 wafer of 4" at a time
PP-bath:
*1-25 wafers of 4" at a time
BHF-bath in cleanroom 3:
*1-25 wafers of 4" at a time
BHF-bath in cleanroom 4:
*1-25 wafers of 4" or 6" at a time
BHF-bath in RCA bench:
*1-25 wafers of 4" or 6" at a time
|
Plastic beaker:
*1-5 wafer of 4" at a time
PP-bath:
*1-25 wafers of 4" at a time
HF-bath in RCA bench:
*1-25 wafers of 4" or 6" at a time
|
1-7 wafer of 4" at a time
|
1-25 wafer of 4" at a time
|-
|'''Size of substrate'''
|
4"-6" wafers
|
2"-6" wafers
|
4" wafers
|
|
4" wafers
|-valign="top"
|'''Allowed materials'''
|
In plastic beaker or PP-bath in the fume hood in cleanroom 2:
*All materials
BHF-bath in cleanroom 3:
*Silicon
*Silicon
*Silicon nitrides
*Poly Silicon
*Silicon oxides
*Silicon Oxide
*Photoresist
*Silicon Nitride
BHF-bath in the RCA bench:
*Silicon Oxynitride
*Only wafers with phosphor glass or boron glass that comes directly from one of the furnaces in stack A.
|
|
In plastic beaker or PP-bath in the fume hood in cleanroom 2:
*All materials
*All materials
HF-bath in RCA bench:
*Only wafers that are being RCA cleaned
|
|
In plastic beaker in the fume hood in cleanroom 2:
*All materials
*All materials
|-
|-style="background:LightGrey; color:black"
!Restrictions
|Wafers have to be cleaned in 7UP or RCA before further processing.
|No wafers with metal are allowed in this bath
|Only for wafers with phosphor glass or boron glass that comes directly from one of the furnaces in stack A. All other substrates and material are strictly forbidden to go into the tank.
|None
|None
|-
|}
<br clear="all" />
==Comparing different HF baths==
{|border="1" cellspacing="1" cellpadding="3" style="text-align:left;"
|-
|-style="background:silver; color:black"
!
! 1% HF in RCA Bench
! 10% HF in D3 wet bench 5 (Oxide etch 3)
! 1% HF Plastic beaker
|-
|-style="background:WhiteSmoke; color:black"
!Batch size!
|1-25 wafers at a time
|1-25 wafer at a time
|1-7 wafers at a time
|-
|-style="background:LightGrey; color:black"
!Size of substrate
|2"-6" wafers
|2"- 6" wafers or any that fits in a dedicated holder
|2"- 4" wafers or any that fits in a dedicated holder
|-
|-style="background:WhiteSmoke; color:black"
!Allowed materials
|Only for wafers that are being RCA cleaned
|All materials
|All materials
|-
|}
<br clear="all" />
==40% HF==
{|border="1" cellspacing="1" cellpadding="2" style="text-align:left;"
|-
|-style="background:silver; color:black"
!
! 40% HF in Plastic beaker, only done by Nanolab staff
|-
|-style="background:WhiteSmoke; color:black"
!Batch size!
|1 wafer at a time
|-
|-style="background:LightGrey; color:black"
!Size of substrate
|Any that fits to a dedicated holder
|-
|-style="background:WhiteSmoke; color:black"
!Allowed materials
|All materials
|-
|}
<br clear="all" />
==BOE 7:1 Etchant VLSI with Surfactant bath==
{|border="1" cellspacing="1" cellpadding="3" style="text-align:left;"
|-
|-style="background:silver; color:black"
!
! BOE 7:1 Etchant VLSI with Surfactant bath
|-
|-style="background:WhiteSmoke; color:black"
!Batch size!
|1-25 wafers at a time
|-
|-style="background:LightGrey; color:black"
!Size of substrate
|4" wafers
|-
|-style="background:WhiteSmoke; color:black"
!Allowed materials
|
|
*Silicon
*Silicon
*Silicon nitrides
*Poly silicon
*Silicon oxides
*Silicon nitrides  
*Silicon oxynitrides
*Silicon oxides  
*Photoresist
*Photoresist
|-
|-style="background:WhiteSmoke; color:black"
!Remark
|
Amorphous silicon can be used as a mask fro SiO2 etching.<br/>
For very long and deep etches of SiO2/Quartz (several hours/micrometers) <br/>
we have indications that show that it is not good to use the BOE 7:1 Etchant VLSI with Surfactant etch. <br/>
The amorphous silicon has small holes (etch pits) which the BOE 7:1 Etchant VLSI with Surfactant etch penetrates and the SiO2 below is etched.
|-
|}
|}
==Life time of the photoresist and blue film in BHF==
Photoresist delaminates from the substrate in BHF. For standard photoresist this process starts after about or less than ½ hour but the time can vary with resist pattern. It starts by under etching the photoresist at the edges. The life time can be prolonged a little to ½ hour - 40 minutes if the photoresist is baked at 120<sup>o</sup>C.
Blue film also has a limited life time in BHF. Blue film is mainly used for back side protecting the wafer while etching on the front side. The life time of Blue film is also about ½ hour.

Latest revision as of 14:31, 15 September 2026

Feedback to this page: click here

Unless anything else is stated, everything on this page, text and pictures are made by DTU Nanolab.

All links to Kemibrug (SDS) and Labmanager Including APV, requires login.

Etch Wet Silicon Oxide Silicon Oxide

Wet Silicon Oxide Etch (BHF, HF and BOE 7:1 Etchant VLSI)

Silicon oxide can be etched using HF. At DTU Nanolab it is mainly used in a buffered version BHF (premixed). You can find safety datasheets on Kemibrug here The BHF has a stable etch rate and is gentle to photoresist due to an almost pH neutral solution which makes photoresist a good masking material for the oxide etch.

BOE 7:1 Etchant VLSI with Surfactant (BHF with wetting agent) can also be used for etching silicon oxide. This is mainly for etching small holes. At DTU Nanolab we do not have BHF with wetting agent in a prepared bath, it's only to be used in fumehoods. It's not very often used and we do not have it as a standard chemical. Please contact DTU Nanolab if you need it.

Wafers with metals or other materials, not allowed in the dedicated oxide etch baths, can be etched using a plastic beaker in Fume hood 01 or 02 (Acids/bases) in D-3. Samples with III-V materials (e.g. InP and GaAs) must be etched in Fume hood 07: III-V Avids/bases in D-3.

The user manual for Oxide etch 1: BHF, APV's and contact information can be found in LabManager by clicking here

The user manual for Oxide etch 2: BHF (clean), APV's and contact information can be found in LabManager by clicking here

The user manual for Oxide etch 3: 10% HF, APV's and contact information can be found in LabManager by clicking here

The user manual for various HF baths in RCA and Fume hoods, APV's and contact information can be found in LabManager by clicking here

Working with HF above 13% is only allowed by Nanolab staff


Process information:
See more etch rates in HF solutions.


Etchant BHF 1% HF / 5% HF / 10% HF 40% HF BOE 7:1 Etchant VLSI with Surfactant
Purpose Etching of silicon oxide
  • Etching of silicon oxide with a stable etch rate
  • Mainly for removing native oxide
  • Mainly for etching deep into borofloat or quartz wafers. Only Nanolab staff are allowed to work with this HF.
  • Etching of silicon oxide - especially for etching small holes
Link to safety APV and SDS (You must be logged in to Kemibrug to view SDSs)
Performance Isotropic
  • Isotropic
  • Isotropic
  • Isotropic
  • Isotropic
Etch rates

See more

  • Wet thermal oxide:75-80nm/min
  • Wet thermal oxide:~6nm/min(1%) / 25nm/min(5%) / 52nm/min(10%)
  • Boronfloat and quartz: ~3-4 μm/min
  • Thermal oxide 80 nm/min
Lifetime of photoresist
  • ~½ hour
  • ~½ hour
  • ~½ hour
  • ~½ hour
Process parameter range Chemical solution
  • BHF (12%HF with Ammoniumflouride)
  • 1% / 5% HF
  • 40% HF
  • BOE 7:1 Etchant VLSI with Surfactant (BHF with a wetting agent)
Temperature
  • Room temperature
  • Room temperature
  • Room temperature
  • Room temperature
Substrates Masking material
  • Silicon nitride
  • Poly silicon
  • Photoresist
  • Blue film
  • Silicon nitride
  • Poly silicon
  • Photoresist delaminates
  • Blue film
  • Photoresist delaminates
  • Silicon nitride (Only on quartz wafers)
  • Poly silicon (Only on quartz wafers)
  • Blue film
  • Chromium and gold
  • Silicon nitride
  • Poly silicon
  • Photoresist
  • Blue film

Life time of the photoresist and blue film in BHF

Photoresist delaminates from the substrate in BHF. For standard photoresist this process starts after about or less than ½ hour but the time can vary with resist pattern. It starts by under etching the photoresist at the edges. The life time can be prolonged a little to ½ hour - 40 minutes if the photoresist is baked at 120oC.

Blue film also has a limited life time in BHF. Blue film is mainly used for back side protecting the wafer while etching on the front side. The life time of Blue film is also about ½ hour.




Comparing different BHF baths

BHF (KOH) in D-3(Oxide etch 1: BHF) BHF clean in D-3 (Oxide etch 2: BHF) BHF in RCA Bench BHF in PP-bath BHF Plastic beaker
Batch size! 1-25 wafers at a time 1-25 wafer at a time 1-25 wafers at a time 1-25 wafers at a time 1-7 wafers at a time
Size of substrate 2"-6" wafers 2"-6" wafers 2"-6" wafers 2"- 4" wafers or any that fits in a dedicated holder 2"- 4" wafers or any that fits in a dedicated holder
Allowed materials
  • Silicon
  • Poly Silicon
  • Silicon Oxide
  • Silicon Nitride
  • Silicon Oxynitride
  • Photoresist
  • Blue film
  • Silicon
  • Poly Silicon
  • Silicon Oxide
  • Silicon Nitride
  • Silicon Oxynitride
  • Photoresist
  • Blue film
  • Silicon
  • Poly Silicon
  • Silicon Oxide
  • Silicon Nitride
  • Silicon Oxynitride
  • All materials
  • All materials
Restrictions Wafers have to be cleaned in 7UP or RCA before further processing. No wafers with metal are allowed in this bath Only for wafers with phosphor glass or boron glass that comes directly from one of the furnaces in stack A. All other substrates and material are strictly forbidden to go into the tank. None None


Comparing different HF baths

1% HF in RCA Bench 10% HF in D3 wet bench 5 (Oxide etch 3) 1% HF Plastic beaker
Batch size! 1-25 wafers at a time 1-25 wafer at a time 1-7 wafers at a time
Size of substrate 2"-6" wafers 2"- 6" wafers or any that fits in a dedicated holder 2"- 4" wafers or any that fits in a dedicated holder
Allowed materials Only for wafers that are being RCA cleaned All materials All materials


40% HF

40% HF in Plastic beaker, only done by Nanolab staff
Batch size! 1 wafer at a time
Size of substrate Any that fits to a dedicated holder
Allowed materials All materials


BOE 7:1 Etchant VLSI with Surfactant bath

BOE 7:1 Etchant VLSI with Surfactant bath
Batch size! 1-25 wafers at a time
Size of substrate 4" wafers
Allowed materials
  • Silicon
  • Poly silicon
  • Silicon nitrides
  • Silicon oxynitrides
  • Silicon oxides
  • Photoresist
Remark

Amorphous silicon can be used as a mask fro SiO2 etching.
For very long and deep etches of SiO2/Quartz (several hours/micrometers)
we have indications that show that it is not good to use the BOE 7:1 Etchant VLSI with Surfactant etch.
The amorphous silicon has small holes (etch pits) which the BOE 7:1 Etchant VLSI with Surfactant etch penetrates and the SiO2 below is etched.