Specific Process Knowledge/Etch/ICP Metal Etcher/Aluminium: Difference between revisions

From LabAdviser
Jml (talk | contribs)
Created page with "=== Aluminium etch === The aluminium etch has two steps: ; Breakthrough : The breakthrough step is designed to break through the native aluminium oxide layer that is present..."
 
Jmli (talk | contribs)
 
(13 intermediate revisions by 4 users not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/ICP_Metal_Etcher/Aluminium click here]'''
<!--Checked for updates on 30/7-2018 - ok/jmli -->
<!--Page reviewed by jmli 9/8-2022  -->
=== Aluminium etch ===
=== Aluminium etch ===
{{Template:Author-jmli1}}
<!--Checked for updates on 2/02-2023 - ok/jmli -->


The aluminium etch has two steps:
The aluminium etch has two steps:
Line 31: Line 37:
|-
|-
! Pressure (mTorr)
! Pressure (mTorr)
| 2,  Strike 3 secs @ 15 mTorr???
| 2,  Strike 3 sec@5 mTorr
| 1
| 1
|-
|-
Line 50: Line 56:
| 30
| 30
|-
|-
!Results
|
|
|-
!Etch rate
|
|~350 nm/min (depending on features size and etch load)
|}
{| border="2" cellpadding="2" cellspacing="1" style="text-align:center;"
|+ '''Al etch''' ''made by Chantal Silvetre@nanolab October 2014''
|-
! rowspan="2" | Parameter
! colspan="2" | Process step
|-
! width="200" | Breakthrough
! width="200" | Main
|-
! Time (secs)
| 20
| 40 (variable)
|-
! HBr (sccm)
| -
| 15
|-
! Cl<sub>2</sub> (sccm)
| 20
| 25
|-
! Pressure (mTorr)
| 2,  Strike 3 secs @ 6 mTorr
| 1
|-
! Coil power (W)
| 600
| 500
|-
! Platen power (W)
| 125
| 100
|-
! Temperature (<sup>o</sup>C)
| 20
| 20
|-
! Spacers (mm)
| 100
| 100
|-
!Results
|
|
|-
!Etch rate
|
|~282 nm/min (depending on features size and etch load)
|}
|}

Latest revision as of 15:11, 2 February 2023

Feedback to this page: click here

Aluminium etch

Unless otherwise stated, all content on this page was created by Jonas Michael-Lindhard, DTU Nanolab

The aluminium etch has two steps:

Breakthrough
The breakthrough step is designed to break through the native aluminium oxide layer that is present on all aluminium surfaces. The duration of this step should remain fixed.
Main
The main step etches bulk aluminium.
Al etch
Parameter Process step
Breakthrough Main
Time (secs) 20 40 (variable)
HBr (sccm) - 15
Cl2 (sccm) 20 25
Pressure (mTorr) 2, Strike 3 sec@5 mTorr 1
Coil power (W) 600 500
Platen power (W) 125 100
Temperature (oC) 20 20
Spacers (mm) 30 30
Results
Etch rate ~350 nm/min (depending on features size and etch load)


Al etch made by Chantal Silvetre@nanolab October 2014
Parameter Process step
Breakthrough Main
Time (secs) 20 40 (variable)
HBr (sccm) - 15
Cl2 (sccm) 20 25
Pressure (mTorr) 2, Strike 3 secs @ 6 mTorr 1
Coil power (W) 600 500
Platen power (W) 125 100
Temperature (oC) 20 20
Spacers (mm) 100 100
Results
Etch rate ~282 nm/min (depending on features size and etch load)