==Results of Design of Experiments optimization of magnetic stack etching ( | '''Feedback to this page''': '''[mailto:plasma@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/IBE%E2%81%84IBSD_Ionfab_300/IBE_magnetic_stack_etch click here]''' | ||
<br> '''''The work on this page was done Kristian Hagsted Rasmussen, DTU Nanolab, unless otherwise stated''''' | |||
=Etching magnetic stacks= | |||
Magnetic stacks can be etched or more precisly milled in the Ion Beam Etcher (IBE). Below is presented some work done on milling stacks of magnetic layers. | |||
==Results of Design of Experiments optimization of magnetic stack etching (Kristian Hagsted Rasmussen@nanotech.dtu.dk spring 2011)== | |||
===Process parameters=== | ===Process parameters=== | ||
| Line 12: | Line 19: | ||
|Neutalizer current [mA] | |Neutalizer current [mA] | ||
|450 | |450 | ||
|450 | |||
|550 | |||
|- | |- | ||
|RF Power [W] | |RF Power [W] | ||
|800 | |800 | ||
| - | |||
| - | |||
|- | |- | ||
|Beam current [mA] | |Beam current [mA] | ||
|400 | |400 | ||
|400 | |||
|500 | |||
|- | |- | ||
|Beam voltage [V] | |Beam voltage [V] | ||
|500 | |500 | ||
|400 | |||
|600 | |||
|- | |- | ||
|Beam accelerator voltage | |Beam accelerator voltage | ||
|500 | |500 | ||
|400 | |||
|600 | |||
|- | |- | ||
|Ar flow to neutralizer [sccm] | |Ar flow to neutralizer [sccm] | ||
|5.0 | |5.0 | ||
| - | |||
| - | |||
|- | |- | ||
|Ar flow to beam [sccm] | |Ar flow to beam [sccm] | ||
|10.0 | |10.0 | ||
| - | |||
| - | |||
|- | |- | ||
|Rotation speed [rpm] | |Rotation speed [rpm] | ||
|20 | |20 | ||
| - | |||
| - | |||
|- | |- | ||
|Stage angle [degrees] | |Stage angle [degrees] | ||
|5 | |5 | ||
|5 | |||
|15 | |||
|- | |- | ||
|Helium backside cooling [Torr] | |Helium backside cooling [Torr] | ||
|37.5 | |37.5 | ||
| - | |||
| - | |||
|- | |- | ||
|} | |} | ||
<br clear="all"/> | |||
===Some SEM profile images of the etched stacks=== | ===Some SEM profile images of the etched stacks=== | ||
| Line 51: | Line 79: | ||
[[image:IBE magnetic stack A3-13.jpg|300x300px|thumb|center|Etched magnetic stack with poor structure transfer, the parameters chosen was clearly not optimal. Chosen etch parameters result in severe trenching]] | [[image:IBE magnetic stack A3-13.jpg|300x300px|thumb|center|Etched magnetic stack with poor structure transfer, the parameters chosen was clearly not optimal. Chosen etch parameters result in severe trenching]] | ||
|} | |} | ||
For a good pattern transfer with IBE a large amount of redeposition on the resist edge has been observed. To reduce this redeposition the best option seems to use a | For a good pattern transfer with IBE a large amount of redeposition on the resist edge has been observed. To reduce this redeposition the best option seems to be to use a photo resist just thick enough for the wanted etch depth. An alternative is sidewall sputtering at low incident angle. However experiments have shown poor cleaning rate and for narrow structures low angles will give rise to shadowing effects. | ||
===Endpoint detection with SIMS=== | ===Endpoint detection with SIMS=== | ||
| Line 59: | Line 87: | ||
|} | |} | ||
End point detection is achieved by SIMS, and the etch rate is approximately 25 Nm/min. | End point detection is achieved by SIMS, and the etch rate is approximately 25 Nm/min. | ||
Resist stripping can be hard due to burned resist, to remedy this try to lower the current. Changing the | |||
===Problems with resists stripping after etching=== | |||
Resist stripping after the etch can be hard due to burned resist, to remedy this try to lower the current. Changing the current will change the sidewall angle and new studies of etch profiles will be necessary. For help, discussion and further info please contact the dry etch group [mailto:dryetch@nanolab.dtu.dk]. | |||
===Design of Experiment results=== | ===Design of Experiment results=== | ||
| Line 73: | Line 104: | ||
* Good end point detection by SIMS. | * Good end point detection by SIMS. | ||
* Burned resist: Lower current, 300 mA can limit resist burning. Note this <b>will</b> affect pattern transfer. | * Burned resist: Lower current, 300 mA can limit resist burning. Note this <b>will</b> affect pattern transfer. | ||
* Hare ears due to redeposition, thinner resist can limit the size. | * Hare ears (also called fences) due to redeposition, thinner resist can limit the size. | ||