==Results from the acceptance test in February 2011== | ==Results from the acceptance test in February 2011== | ||
'''Acceptance test for Ti etch:''' | '''Acceptance test for Ti etch :''' | ||
{| border="2" cellspacing="0" cellpadding="2" | {| border="2" cellspacing="0" cellpadding="2" | ||
|- | |- | ||
| Line 12: | Line 15: | ||
*50 mm SSP Si wafer | *50 mm SSP Si wafer | ||
*525 µm thick | *525 µm thick | ||
*Supplied by | *Supplied by Nanolab | ||
|. | |. | ||
|- | |- | ||
| Line 29: | Line 32: | ||
!style="background:silver; color:black" align="left" valign="top"|Features to be etched | !style="background:silver; color:black" align="left" valign="top"|Features to be etched | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
* | *300 nm - 3µm dots and lines + a square of 200µmx200µm | ||
|. | |. | ||
|- | |- | ||
!style="background:silver; color:black" align="left" valign="top"|Etch depth | !style="background:silver; color:black" align="left" valign="top"|Etch depth | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
* | *300nnm | ||
| | | | ||
*~270 nm | *~270 nm | ||
| Line 40: | Line 43: | ||
!style="background:silver; color:black" align="left" valign="top"|Etch rate | !style="background:silver; color:black" align="left" valign="top"|Etch rate | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
*> | *>80 nm/min | ||
| | | | ||
* | *22 nm/min +- 0.3nnm/min (one standard deviation) | ||
|- | |- | ||
!style="background:silver; color:black" align="left" valign="top"|Etch rate uniformity | !style="background:silver; color:black" align="left" valign="top"|Etch rate uniformity | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
*< | *<±2% | ||
| | | | ||
* | *±(0.2% ±0.2%) | ||
|- | |- | ||
!style="background:silver; color:black" align="left" valign="top"|Reproducibility | !style="background:silver; color:black" align="left" valign="top"|Reproducibility | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
*< | *<±2% | ||
| | | | ||
* | *±(0.8% ±0.5%) | ||
|- | |- | ||
!style="background:silver; color:black" align="left" valign="top"|Selectivity ( | !style="background:silver; color:black" align="left" valign="top"|Selectivity (Ti etch rate/ZEP etch rate) | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
*At least 1:1 | *At least 1:1 | ||
| Line 75: | Line 78: | ||
!Ti etch acceptance | !Ti etch acceptance | ||
|- | |- | ||
| | |Neutralizer current [mA] | ||
|550 | |550 | ||
|- | |- | ||