Jump to content

Specific Process Knowledge/Thin film deposition/Deposition of Vanadium Silicide/V3Si RF-DC Co-Sputtering in Cluster Lesker PC3: Difference between revisions

From LabAdviser
Eves (talk | contribs)
Created page with "<i>This page is written by <b>Evgeniy Shkondin @ DTU Nanolab</b> if nothing else is stated.<br> All images and data on this page belong to <b>DTU Nanolab</b>.<br> The exploratory deposition and characterization described below were performed in <b>2025</b>.<br></i> =Exploratory V-Si RF-DC co-sputtering in Cluster Lesker PC3= This page documents an early, non-systematic attempt to deposit vanadium silicide by simultaneous RF sputtering of a 4-inch Si target and DC sputt..."
 
Eves (talk | contribs)
 
(3 intermediate revisions by the same user not shown)
Line 5: Line 5:
=Exploratory V-Si RF-DC co-sputtering in Cluster Lesker PC3=
=Exploratory V-Si RF-DC co-sputtering in Cluster Lesker PC3=


This page documents an early, non-systematic attempt to deposit vanadium silicide by simultaneous RF sputtering of a 4-inch Si target and DC sputtering of a 3-inch V target in the <i>Cluster Lesker PC3</i> chamber. Two otherwise nominally identical depositions were compared: one without RF substrate bias and one with 30 W RF substrate bias.
This page documents an <b>early</b>, <b>non-systematic attempt</b> to deposit vanadium silicide by simultaneous RF sputtering of a 4-inch Si target and DC sputtering of a 3-inch V target in the <i>Cluster Lesker PC3</i> chamber. Two otherwise nominally identical depositions were compared: one without RF substrate bias and one with 30 W RF substrate bias.
 
We achieved the expected results for the V<sub>3</sub>Si process in PC1 and describe them [[Specific Process Knowledge/Thin film deposition/Deposition of Vanadium Silicide/V3Si RF-DC Co-Sputtering in Cluster Lesker PC1|in dedicated page]].


The experiment gave a striking result. In the measured 30–80&deg; GiXRD range, the unbiased sample showed only reflections assigned to cubic A15 V<sub>3</sub>Si, whereas the sample deposited with 30 W RF substrate bias showed only reflections assigned to hexagonal C40 VSi<sub>2</sub>. The two samples also had very different surface morphologies and sheet resistances.
The experiment gave a striking result. In the measured 30–80&deg; GiXRD range, the unbiased sample showed only reflections assigned to cubic A15 V<sub>3</sub>Si, whereas the sample deposited with 30 W RF substrate bias showed only reflections assigned to hexagonal C40 VSi<sub>2</sub>. The two samples also had very different surface morphologies and sheet resistances.
Line 177: Line 179:
! XRR density
! XRR density
! XRR roughness
! XRR roughness
! Sheet resistance
 
! Calculated resistivity
|-
|-
| No substrate bias
| No substrate bias
Line 186: Line 187:
| 4.741 g/cm<sup>3</sup>
| 4.741 g/cm<sup>3</sup>
| 7.873 nm
| 7.873 nm
| 29.34 &Omega;/sq
 
| 276 &micro;&Omega;&middot;cm
|-
|-
| 30 W RF substrate bias (69 V DC bias)
| 30 W RF substrate bias (69 V DC bias)
Line 195: Line 195:
| Not obtained
| Not obtained
| Not obtained
| Not obtained
| 6.64 &Omega;/sq
| Not calculated because thickness is unknown
|}
|}


Line 298: Line 296:
The 30 W RF-biased film was too rough for a defensible XRR model. No thickness, density, roughness or resistivity should be quoted from this scan. A cross-sectional measurement is needed.
The 30 W RF-biased film was too rough for a defensible XRR model. No thickness, density, roughness or resistivity should be quoted from this scan. A cross-sectional measurement is needed.


=SEM surface morphology=
=Further characterization and data access=
 
<gallery caption="" widths="800px" heights="570px" perrow="1">
image:eves_SEM_V3Si_PC3_bias_comparison_20260916.png|Plan-view SEM comparison at 200,000&times; and 300,000&times;. Original scale bars and microscope metadata are preserved in each panel.
</gallery>
 
Both films are rough and polycrystalline, but the morphologies differ strongly:
 
* the unbiased V<sub>3</sub>Si film consists mainly of much finer, densely distributed granular/nodular surface features, with occasional brighter agglomerates;
* the 30 W-biased VSi<sub>2</sub> film contains substantially larger faceted plate-like grains, many with visible terraces or banded surface contrast;
* the coarser faceted morphology of the biased sample is consistent with its strongly damped XRR response, but plan-view SEM cannot provide an RMS roughness or film thickness.
 
=Electrical results=
 
The unbiased V<sub>3</sub>Si sample had a sheet resistance of 29.34 &Omega;/sq. Combining this value with the XRR thickness gives:
 
<math>
\rho=R_s t
=29.34\ \Omega/\square \times 94.046\ \mathrm{nm}
=276\ \mu\Omega\cdot\mathrm{cm}
</math>
 
The 30 W-biased VSi<sub>2</sub> sample had a much lower sheet resistance of 6.64 &Omega;/sq, but this does <b>not</b> by itself demonstrate a lower material resistivity or a better film. Sheet resistance depends on both resistivity and thickness. The biased layer may be considerably thicker because of reaction with the Si wafer, may contain an electrically parallel interfacial/unreacted layer, or may simply have a different intrinsic resistivity and connectivity. Until its thickness and cross-sectional structure are measured, only the sheet resistance should be reported.
 
=Interpretation of the bias-induced phase change=
 
The most likely working interpretation is that the oxide-stripped Si substrate was an active reactant and that RF substrate bias changed the early interface reaction sufficiently to select a different silicide phase.
 
# <b>The targets supplied a V-rich flux.</b> The estimated target-derived atomic ratio was V:Si = 4.22, which is more V-rich than V<sub>3</sub>Si. Formation of V<sub>3</sub>Si in the unbiased sample therefore requires some Si uptake from the wafer, but only a modest amount: approximately 11.7 nm of substrate-equivalent Si in the simple full-retention mass balance.
# <b>Bare crystalline Si provides a very large Si reservoir.</b> Earlier V/Si interface studies report that VSi<sub>2</sub> is the first silicide phase to nucleate and grow at a single-crystal Si/V interface. More recent V<sub>3</sub>Si work likewise shows that limiting the available Si favors the V-rich A15 phase, whereas an unrestricted Si supply favors Si-rich silicides.
# <b>The unbiased run may have formed an early V<sub>3</sub>Si-rich reaction layer.</b> With the V-rich incoming flux, such a layer could kinetically limit further Si transport from the wafer and preserve the A15 phase during the remainder of the 1200 s deposition.
# <b>The 69 V substrate DC bias introduced energetic ion bombardment.</b> Ion bombardment can increase defect generation, surface mobility, atomic mixing and re-sputtering. In this experiment it may have disrupted or delayed formation of the V<sub>3</sub>Si-rich barrier, enhanced access to substrate Si, and allowed the thermodynamically/kinetically favored Si-rich VSi<sub>2</sub> reaction to continue. This is a plausible mechanism, not a direct measurement.
# <b>The bias also changed the plasma state.</b> The Si display changed from 100 to 110 V and the V discharge voltage from 322 to 309 V at fixed applied target powers. The actual V and Si arrival rates may therefore have shifted relative to the separate elemental calibrations. Voltage alone is insufficient to calculate the change in composition.
 
The data demonstrate that 30 W RF substrate bias is not a small microstructural adjustment for this process. On HF-stripped Si at 600 &deg;C it changes the detected crystalline product from V<sub>3</sub>Si to VSi<sub>2</sub> and produces a much coarser surface morphology.
 
=Limitations=
 
* Only two depositions were compared; there is no bias-power series and no repeatability test.
* The elemental deposition rates were measured separately, not simultaneously during co-sputtering at 600 &deg;C.
* No direct V:Si composition measurement is available.
* GiXRD establishes crystalline phase identity within its detection limits but does not quantify amorphous material or reliable phase fractions.
* The biased sample has no measured thickness; therefore its resistivity and true deposition/reaction rate are unknown.
* Plan-view SEM does not reveal the film/substrate interface or how much Si was consumed.
* The influence of the HF-to-load delay and any regrown interfacial oxide was not isolated.
* Phase-pure A15 diffraction does not by itself prove superconductivity; a temperature-dependent resistance measurement is required.
 
=References=
 
* W. Zhang et al., “Thin-film synthesis of superconductor-on-insulator A15 vanadium silicide,” <i>Scientific Reports</i> 11, 2358 (2021), [https://doi.org/10.1038/s41598-021-82046-1 DOI: 10.1038/s41598-021-82046-1]. This work discusses control of Si supply during V<sub>3</sub>Si formation and provides the V/Si molar-volume calculation used as a cross-check here.
* R. J. Schutz et al., “The formation of vanadium silicides at thin-film interfaces,” <i>Journal of Applied Physics</i> 50, 5773–5781 (1979), [https://doi.org/10.1063/1.326718 DOI: 10.1063/1.326718]. This study reports VSi<sub>2</sub> as the first silicide phase to nucleate and grow at single-crystal Si/V interfaces.
* M. Bose et al., “In-situ Investigation of the Phase Formation and Superconductivity in V<sub>3</sub>Si Thin Films at High Temperatures,” [https://arxiv.org/abs/2412.04159 arXiv:2412.04159]. This work shows that interface/barrier consumption and excessive Si access can drive formation of undesirable Si-rich silicides.
* M. Manzo-Perez et al., “Substrate effects on phase formation and interfacial stability in superconducting vanadium silicide thin films,” <i>Applied Physics Letters</i> 127, 122601 (2025), [https://doi.org/10.1063/5.0291576 DOI: 10.1063/5.0291576].


[[Category:Thin film deposition]]
SEM images, electrical properties, sheet resistances, and the complete integrated interpretation are available on the corresponding <b>LabIntra page</b> or upon request. Please contact <b>Evgeniy Shkondin, DTU Nanolab</b>, for further details and results.
[[Category:Sputtering]]
[[Category:Vanadium silicide]]
[[Category:Cluster Lesker PC3]]

Latest revision as of 18:57, 13 October 2026

This page is written by Evgeniy Shkondin @ DTU Nanolab if nothing else is stated.
All images and data on this page belong to DTU Nanolab.
The exploratory deposition and characterization described below were performed in 2025.

Exploratory V-Si RF-DC co-sputtering in Cluster Lesker PC3

This page documents an early, non-systematic attempt to deposit vanadium silicide by simultaneous RF sputtering of a 4-inch Si target and DC sputtering of a 3-inch V target in the Cluster Lesker PC3 chamber. Two otherwise nominally identical depositions were compared: one without RF substrate bias and one with 30 W RF substrate bias.

We achieved the expected results for the V3Si process in PC1 and describe them in dedicated page.

The experiment gave a striking result. In the measured 30–80° GiXRD range, the unbiased sample showed only reflections assigned to cubic A15 V3Si, whereas the sample deposited with 30 W RF substrate bias showed only reflections assigned to hexagonal C40 VSi2. The two samples also had very different surface morphologies and sheet resistances.

This PC3 experiment is separate from the later, systematic V3Si process-development study performed in PC1.


Substrate and deposition conditions

  • Substrate: 150 mm Si(100) wafer
  • Surface preparation: native SiO2 removed by HF immediately before deposition
  • Si source: 4-inch Si target, RF sputtering
  • V source: 3-inch V target, DC sputtering
  • Working pressure: 3 mTorr
  • Deposition temperature: 600 °C
  • Deposition time: 1200 s
  • Substrate-bias comparison: no RF bias versus 30 W RF bias
  • Recorded DC substrate-bias voltage at 30 W RF bias: 69 V
PC3 V-Si co-sputtering conditions
Condition Si target Si power Displayed Si voltage V target V power Displayed V voltage Pressure RF substrate power Substrate DC bias Temperature Time
No substrate bias 4-inch Si 120 W RF 100 V 3-inch V 100 W DC 322 V 3 mTorr 0 W Not applied 600 °C 1200 s
30 W RF substrate bias 4-inch Si 120 W RF 110 V 3-inch V 100 W DC 309 V 3 mTorr 30 W 69 V 600 °C 1200 s

Although the applied target powers were unchanged, the displayed Si and V discharge voltages changed when the substrate RF bias was enabled. This shows that the plasma impedance/coupling was not identical in the two runs. Consequently, the elemental rates measured in separate calibration depositions should be treated as nominal flux estimates rather than exact in-situ co-deposition rates.

Power calibration and estimated V:Si atomic-arrival ratio

The individual elemental deposition rates measured at 3 mTorr were:

Individual elemental-rate calibration
Element Target size Mode Power Pressure Pure-element thickness rate Density used Molar mass used
Si 4 inch RF 120 W 3 mTorr 0.024 nm/s 2.329 g/cm3 28.0855 g/mol
V 3 inch DC 100 W 3 mTorr 0.0700 nm/s 6.11 g/cm3 50.9415 g/mol

The thickness-rate ratio was therefore:

rVrSi=0.07000.024=2.92

This number cannot be compared directly with the 3:1 atomic stoichiometry of V3Si. For an elemental rate calibration, the atomic arrival rate is proportional to:

Φi∝ρiriMi

where ρi is the elemental density, ri is the pure-element thickness rate, and Mi is the molar mass. The nominal target-derived atomic-arrival ratio is consequently:

ΦVΦSi=ρVrV/MVρSirSi/MSi=4.22

Thus, the flux supplied by the two targets was nominally about 80.8 at.% V and 19.2 at.% Si, corresponding to V4.22Si rather than V3Si. The pure-element thickness-rate ratio required for an atomic V:Si ratio of 3 is approximately:

(rVrSi)V3Si=3MV/ρVMSi/ρSi=2.07

The calibrated target flux was therefore substantially more V-rich than the ideal V3Si value. The formation of V3Si in the unbiased sample cannot be explained by the target flux alone; Si supplied by the oxide-stripped Si wafer must be considered.

Simple target/substrate mass balance

Using the calibrated rates and 1200 s deposition time, and assuming for the moment that all deposited V was retained:

  • formation of V3Si requires approximately 11.7 nm of substrate-equivalent Si in addition to the Si supplied by the target;
  • the corresponding full-retention V3Si layer thickness is approximately 105 nm using a bulk V3Si density of 5.77 g/cm3;
  • the measured no-bias XRR thickness was 94.046 nm, about 89% of this simple mass-balance value.

The agreement is reasonable for separately calibrated rates, compound formation, a simplified XRR model, and a process performed at 600 °C. It supports substrate participation but is not an independent composition measurement.

If all calibrated V instead formed VSi2, the limiting mass balance would require approximately 214 nm of additional substrate-equivalent Si and would produce roughly 244 nm of VSi2 using a density of 4.42 g/cm3. These are not measured values for the biased sample. They illustrate that formation of VSi2 throughout the deposited material would require extensive Si uptake from the wafer, a change in retained V flux, or both.

Characterization methods

X-ray reflectivity (XRR)

XRR measurements were performed using a Rigaku SmartLab X-ray diffractometer. The Cu X-ray tube was operated at 40 kV and 30 mA. The incident optics included an IPS (incident parallel-slit) adapter with a 5° Soller slit. The slit configuration was IS = 0.05 mm, RS1 = 0.05 mm and RS2 = 0.075 mm. The programmed scan used a step size of 0.01° and a counting time of 2 s per point. The MATLAB analysis reads the actual exported angular coordinates and does not assume a fixed data interval.

Grazing-incidence X-ray diffraction (GiXRD)

GiXRD measurements were performed using the Rigaku SmartLab instrument with a Cu sealed X-ray tube operated at 40 kV and 30 mA. The scans covered 30–80° in 2θ, using a 0.5 mm incident slit, a step size of 0.01° and a scan speed of 2°/min. The incident angle was fixed at ω=2∘ relative to the sample surface.

The shallow fixed incidence increases the film contribution relative to a conventional symmetric scan. Phase assignment is based on the observed reflection series. Reported lattice parameters are approximate because the scans were not subjected to a full instrumental-zero/refraction refinement and the sealed-tube spectrum can contain unresolved Cu Kα contributions.

Scanning electron microscopy (SEM)

Plan-view SEM images were recorded at 5.00 kV with the InLens detector. Images were acquired at 200,000× and 300,000× magnification. The original scale bars and acquisition metadata are retained in the TIFF images.

Sheet resistance

Room-temperature sheet resistance was measured for both samples. Resistivity is calculated only for the unbiased sample because only that sample has a defensible XRR thickness.

Results overview

Measured and fitted results
Condition Crystalline phase detected by GiXRD Lattice parameters from GiXRD XRR thickness XRR density XRR roughness
No substrate bias V3Si, cubic A15 a=4.731±0.003 Å1 94.046 nm 4.741 g/cm3 7.873 nm
30 W RF substrate bias (69 V DC bias) VSi2, hexagonal C40 a=4.574 Å, c=6.376 Å1 Not obtained; surface too rough for a defensible fit Not obtained Not obtained

1 Values are derived from pseudo-Voigt fits to several assigned GiXRD reflections using Cu Kα1 = 1.540593 Å. They should be regarded as approximate GiXRD lattice parameters, not high-resolution lattice refinements.

Grazing-incidence X-ray diffraction results

Unbiased film: A15 V3Si

The unbiased sample contains the characteristic A15 V3Si reflection series. The main fitted peaks are:

Reflection Fitted 2θ Approximate apparent coherence length2
V3Si (200) 38.03° 13.0 nm
V3Si (210) 42.70° 10.8 nm
V3Si (211) 46.99° 14.4 nm
V3Si (320) 71.95° 16.8 nm
V3Si (321) 75.00° 12.5 nm

The mean cubic lattice parameter obtained from the five reflections is a=4.731±0.003 Å. This is slightly larger than the commonly reported room-temperature bulk value of approximately 4.72 Å, but the difference is too small to interpret confidently without a zero-shift/reference correction and a dedicated high-resolution scan.

30 W RF-biased film: C40 VSi2

The biased sample contains the reflection series expected for C40 VSi2. The fitted peaks used for the lattice calculation are:

Reflection Fitted 2θ Comment
VSi2 (110) 39.43° Isolated peak
VSi2 (111) 41.96° Fitted together with (003)
VSi2 (003) 42.50° Fitted together with (111)
VSi2 (112) 48.98° Several C40 reflections are close in this region
VSi2 (031) 73.12° High-angle constraint
VSi2 (032) 78.32° High-angle constraint

A simultaneous least-squares solution of the hexagonal d-spacing relation gives a=4.574 Å and c=6.376 Å, in good agreement with reported C40 VSi2 lattice parameters.

In both samples, “single phase” means that no other crystalline phase was resolved above the detection/background limit within the measured 30–80° range. The scans do not exclude amorphous material, a thin interfacial phase, or a minor crystalline fraction hidden by peak overlap.

2 The coherence lengths are Scherrer estimates based on uncorrected fitted FWHM values. Instrumental broadening, microstrain, texture, peak overlap, and the Cu Kα doublet were not separated. These numbers are therefore approximate coherent-domain sizes and must not be equated directly with SEM surface-feature size.

X-ray reflectivity results

The unbiased sample could be represented by a simplified single vanadium-silicide layer on Si:

  • thickness: 94.046 nm;
  • fitted density: 4.741 g/cm3;
  • fitted layer roughness: 7.873 nm;
  • thickness-derived growth rate: 0.0784 nm/s.

The fitted density is about 82% of the 5.77 g/cm3 bulk value used for V3Si. This can reflect porosity/voids, oxidation, model-density/roughness correlation, lateral non-uniformity, or a more complicated interface than the one-layer model. XRR density alone is not a chemical-composition measurement.

The 30 W RF-biased film was too rough for a defensible XRR model. No thickness, density, roughness or resistivity should be quoted from this scan. A cross-sectional measurement is needed.

Further characterization and data access

SEM images, electrical properties, sheet resistances, and the complete integrated interpretation are available on the corresponding LabIntra page or upon request. Please contact Evgeniy Shkondin, DTU Nanolab, for further details and results.