Specific Process Knowledge/Lithography/Aligners/MAvsMLA: Difference between revisions
Appearance
No edit summary |
|||
| (8 intermediate revisions by the same user not shown) | |||
| Line 15: | Line 15: | ||
Mask design used in the investigation: [[Media:LithoTestAlign 2025 v10.gds|LithoTestAlign_2025_v10.gds]] | Mask design used in the investigation: [[Media:LithoTestAlign 2025 v10.gds|LithoTestAlign_2025_v10.gds]] | ||
<br clear="all" /> | |||
=Tools used in the investigation= | |||
*Wafers | |||
**100mm Si, SSP <100> | |||
*Resists | |||
**[[Specific_Process_Knowledge/Lithography/5214E|AZ 5214E]] (image reversal resist, but processed positive) | |||
**[[Specific_Process_Knowledge/Lithography/MiR|AZ MiR 701]] (positive tone resist) | |||
**[[Specific_Process_Knowledge/Lithography/nLOF|AZ nLOF 2020]] (negative tone resist) | |||
*Spin coating (incl. HMDS) | |||
**[[Specific_Process_Knowledge/Lithography/Coaters#Spin_Coater:_Gamma_UV|Spin Coater: Gamma UV]] | |||
*Exposure | |||
**[[Specific_Process_Knowledge/Lithography/UVExposure/aligner_MA6-2|Aligner: MA6-2]] | |||
**[[Specific_Process_Knowledge/Lithography/UVExposure/aligner_MA6-1|Aligner: MA6-1]] (in PolyFabLab) | |||
**[[Specific Process Knowledge/Lithography/UVExposure/aligner_MLA2|Aligner: Maskless 02]] | |||
**[[Specific Process Knowledge/Lithography/UVExposure/aligner_MLA1|Aligner: Maskless 01]] | |||
*Development (incl. PEB, if relevant) | |||
**[[Specific_Process_Knowledge/Lithography/Development/UV_developer|Developer: TMAH UV-lithography]] | |||
*Inspection | |||
**[[Specific_Process_Knowledge/Characterization/Optical_microscope|Microscope Olympus MX63]] | |||
**[[Specific_Process_Knowledge/Characterization/SEM_Supra_1|SEM Supra 1]] | |||
**[[Specific_Process_Knowledge/Characterization/SEM_Supra_3|SEM Supra 3]] | |||
<br clear="all" /> | |||
=Data from the investigation= | =Data from the investigation= | ||
<!-- <span style="background:#FF2800">THIS PAGE IS UNDER CONSTRUCTION</span>[[image:Under_construction.png|200px]] | <!-- <span style="background:#FF2800">THIS PAGE IS UNDER CONSTRUCTION</span>[[image:Under_construction.png|200px]] | ||
--> | --> | ||
<br clear="all" /> | |||
==AZ 5214E== | ==AZ 5214E== | ||
<br clear="all" /> | |||
===Resolution (AZ 5214E)=== | ===Resolution (AZ 5214E)=== | ||
<br clear="all" /> | <br clear="all" /> | ||
| Line 284: | Line 307: | ||
====Linewidth and sidewall angle vs defocus parameter (AZ 5214E)==== | ====Linewidth and sidewall angle vs defocus parameter (AZ 5214E)==== | ||
<br clear="all" /> | <br clear="all" /> | ||
'''Result of image analysis of SEM images of 2µm triplets:''' | '''Result of image analysis of SEM images of 2µm triplets:''' | ||
| Line 338: | Line 360: | ||
==AZ MiR 701== | ==AZ MiR 701== | ||
<br clear="all" /> | |||
===Resolution (AZ MiR 701)=== | ===Resolution (AZ MiR 701)=== | ||
<br clear="all" /> | |||
'''Resolution at optimal processing conditions for 1.5µm AZ MiR 701 using different exposure equipment:''' | '''Resolution at optimal processing conditions for 1.5µm AZ MiR 701 using different exposure equipment:''' | ||
{| class="wikitable" | {| class="wikitable" | ||
| Line 539: | Line 561: | ||
==AZ nLOF 2020== | ==AZ nLOF 2020== | ||
<br clear="all" /> | |||
===Resolution (AZ nLOF 2020)=== | ===Resolution (AZ nLOF 2020)=== | ||
<br clear="all" /> | <br clear="all" /> | ||
'''Resolution at optimal processing conditions for 2µm AZ nLOF 2020 using different exposure equipment:''' | '''Resolution at optimal processing conditions for 2µm AZ nLOF 2020 using different exposure equipment:''' | ||
{| class="wikitable" | {| class="wikitable" | ||
| Line 670: | Line 692: | ||
===Resist profile (AZ nLOF 2020)=== | ===Resist profile (AZ nLOF 2020)=== | ||
<br clear="all" /> | <br clear="all" /> | ||
====Linewidth and sidewall angle vs exposure dose (AZ nLOF 2020)==== | ====Linewidth and sidewall angle vs exposure dose (AZ nLOF 2020)==== | ||
<br clear="all" /> | <br clear="all" /> | ||
'''Result of image analysis of SEM images of 2µm triplets:''' | '''Result of image analysis of SEM images of 2µm triplets:''' | ||
| Line 762: | Line 782: | ||
====Linewidth and sidewall angle vs defocus parameter (AZ nLOF 2020)==== | ====Linewidth and sidewall angle vs defocus parameter (AZ nLOF 2020)==== | ||
<br clear="all" /> | <br clear="all" /> | ||
'''Result of image analysis of SEM images of 2µm triplets:''' | '''Result of image analysis of SEM images of 2µm triplets:''' | ||