Specific Process Knowledge/Etch/DRIE-Pegasus/Pegasus-4/Silicon Nitride Etch: Difference between revisions
Appearance
No edit summary |
|||
| (2 intermediate revisions by the same user not shown) | |||
| Line 48: | Line 48: | ||
====Etch rate & uniformity==== | ====Etch rate & uniformity==== | ||
'''Recipe: ''Slowetch 2''''' | |||
'''SRN (LPCVD) etch uniformity on 6″ wafer | '''SRN (LPCVD) etch uniformity on 6″ wafer''' | ||
[[File:slowetch2_100% loadSRN.png|400px|left|thumb|Process: No mask, 100 % load, etching was done after 10 mins chamber clean + 5 mins TDESC clean (for all wafers)]] | [[File:slowetch2_100% loadSRN.png|400px|left|thumb|Process: No mask, 100 % load, etching was done after 10 mins chamber clean + 5 mins TDESC clean (for all wafers)]] | ||
[[File:slowetch2_100% loadSRN_etchrate.png|400px|left|thumb|Note: etch rate for SRN with Slowetch 2. The 4 wafers were processed on 4 different days, the variation suggests process instability or chamber memory effects influencing etch behavior across runs.]] | [[File:slowetch2_100% loadSRN_etchrate.png|400px|left|thumb|Note: etch rate for SRN with Slowetch 2. The 4 wafers were processed on 4 different days, the variation suggests process instability or chamber memory effects influencing etch behavior across runs.]] | ||
| Line 82: | Line 83: | ||
<br clear="all" /> | <br clear="all" /> | ||
'''SRN (LPCVD) etch uniformity on 6″ wafer | |||
'''Recipe: ''Slowetch''''' | |||
'''SRN (LPCVD) etch uniformity on 6″ wafer ''' | |||
[[File:SRN_slowetch_data_100%load.png|400px|left|thumb|Process: No mask, 100 % load, etching was done after 10 mins chamber clean + 5 mins TDESC clean (for all wafers)<br/> | [[File:SRN_slowetch_data_100%load.png|400px|left|thumb|Process: No mask, 100 % load, etching was done after 10 mins chamber clean + 5 mins TDESC clean (for all wafers)<br/> | ||
| Line 88: | Line 92: | ||
<br clear="all" /> | |||
'''With DUV mask on ~300 nm SRN layer''' | |||
[[File:SRN_slowetch_profilealong center.png|800px|left|thumb|Process: ''Slowetch recipe for 10 mins'', DUV mask (with Barc) ~750 nm, etching was done after 10 mins chamber clean + 5 mins TDESC clean (for all wafers)<br/> | |||
Note: The SEM images illustrate the etched SRN profiles across the wafer, progressing from one edge (left) through the center chip (middle) to the opposite edge (right), the etch rate is ~28 nm/min.]] | |||
Latest revision as of 15:34, 28 July 2025
Feedback to this page: click here
THIS PAGE IS UNDER CONSTRUCTION
Silicon Nitride Recipe
| Parameter | Recipe name: Slow Etch | Recipe name: Slow Etch2 |
|---|---|---|
| Coil Power [W] | 350 | 200 |
| Platen Power [W] | 25 | 50 |
| Platen temperature [oC] | 20 | 20 |
| H2 flow [sccm] | 15 | 15 |
| CF4 flow [sccm] | 30 | 30 |
| Pressure [mTorr] | 3 | 10 |
Etch rate & uniformity
Recipe: Slowetch 2
SRN (LPCVD) etch uniformity on 6″ wafer



Recipe: Slowetch
SRN (LPCVD) etch uniformity on 6″ wafer

Note: The slowetch recipe has faster etch recipe significantly improves etch rate (~30 nm/min) but leads to reduced uniformity (~2.5%) compared to the slower recipes (<1% uniformity). This highlights a trade-off between throughput and etch uniformity in SRN processing.
With DUV mask on ~300 nm SRN layer

Note: The SEM images illustrate the etched SRN profiles across the wafer, progressing from one edge (left) through the center chip (middle) to the opposite edge (right), the etch rate is ~28 nm/min.
*The process was repeated twice, but only one set of data is presented here.