'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Gold click here]''' | '''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Gold click here]''' | ||
Gold can be deposited by e-beam evaporation or sputtering. In the chart below you can compare the different deposition equipment. We also describe the temperature rise on the wafer during gold deposition, the adhesion layers that can be used for gold deposition, the roughness of gold deposited in the Wordentec, and issues with particulates on the gold films in the Temescal and the Wordentec. | Gold can be deposited by e-beam evaporation or sputtering. In the chart below you can compare the different deposition equipment. We also describe the temperature rise on the wafer during gold deposition, the adhesion layers that can be used for gold deposition, the roughness of gold deposited in the Wordentec, and issues with particulates on the gold films in the Temescal and the Wordentec. | ||
| Line 39: | Line 37: | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
! Layer thickness | ! Layer thickness | ||
|10 Å to | |10 Å to 600 nm * | ||
|10 Å to 200 nm | |10 Å to 200 nm | ||
|10 Å to 500 nm | |10 Å to 500 nm * | ||
|10 Å to 500 nm | |10 Å to 500 nm * | ||
| very thin, few nm range | | very thin, few nm range | ||
| very thin, few nm range | | very thin, few nm range | ||
| Line 49: | Line 47: | ||
|-style="background:LightGrey; color:black" | |-style="background:LightGrey; color:black" | ||
! Deposition rate | ! Deposition rate | ||
| | |1-5 Å/s | ||
|1 Å/s (can be adjusted to around 5 Å/s) | |1 Å/s (can be adjusted to around 5 Å/s) | ||
|Depends on process parameters, 1-10 Å/s | |Depends on process parameters, 1-10 Å/s | ||
| Line 87: | Line 85: | ||
|-style="background:LightGrey; color:black" | |-style="background:LightGrey; color:black" | ||
!Heating | |||
|to 250 C (in 10-pocket evaporator) | |||
|no | |||
|no | |||
|to 600 C | |||
|no | |||
|no | |||
|-style="background:WhiteSmoke; color:black" | |||
!Allowed materials | !Allowed materials | ||
| Line 111: | Line 119: | ||
* All samples allowed in the SEM Supra 2 or 3 | * All samples allowed in the SEM Supra 2 or 3 | ||
|-style="background: | |-style="background:LightGrey; color:black" | ||
! Comment | ! Comment | ||
| | | | ||
* Pumpdown approx 20 min. | * Pumpdown approx 20 min. | ||
| | | | ||
| Line 133: | Line 140: | ||
''' | '''*''' ''For thicknesses above 200 nm write to metal@nanolab.dtu.dk as extra deposition costs a higher fee.'' | ||
== Resistive thermal evaporation of Au == | == Resistive thermal evaporation of Au == | ||
| Line 216: | Line 221: | ||
|- | |- | ||
| | | | ||
*[http://labmanager.dtu.dk/d4Show.php?id=5862&mach=429 QC procedure | TiAu or CrAu is tested approximately once a month on both of Nanolab's e-beam evaporators. | ||
*[https://labmanager.dtu.dk/view_binary.php?type=data&mach=429 | |||
'''You can find the QC procedures and data in LabManager here''' (requires login): | |||
*[http://labmanager.dtu.dk/d4Show.php?id=5862&mach=429 QC procedure, E-beam Evaporator (Temescal)]<br> | |||
*[https://labmanager.dtu.dk/view_binary.php?type=data&mach=429 Newest QC data, E-beam Evaporator (Temescal)]<br> | |||
*[http://labmanager.dtu.dk/d4Show.php?id=5862&mach=511 QC procedure, E-beam Evaporator (10-pockets)]<br> | |||
*[https://labmanager.dtu.dk/view_binary.php?type=data&mach=511 Newest QC data, E-beam Evaporator (10-pockets)]<br> | |||
{| {{table}} | {| {{table}} | ||
| align=" | | align="left" valign="top"| | ||
{| border=" | {| border="2" cellspacing="1" cellpadding="2" align="left" style="width:400px" | ||
! QC Recipe: | ! QC Recipe: | ||
! Standard recipes/TiAu or Cr/Au | ! Standard recipes/TiAu or Cr/Au | ||
| Line 239: | Line 249: | ||
|- | |- | ||
|} | |} | ||
| align=" | |- | ||
{| border="2" cellspacing="1" cellpadding="2" align=" | |} | ||
{| {{table}} | |||
| align="left" valign="top"| | |||
{| border="2" cellspacing="1" cellpadding="2" align="left" style="width:400px" | |||
!QC limits | !QC limits | ||
!Both e-beam evaporators | !Both e-beam evaporators | ||
| Line 256: | Line 271: | ||
|- | |- | ||
|} | |} | ||
Thickness is measured in 5 points with a stylus profiler. <br> | Thickness is measured in 5 points with a stylus profiler. <br> | ||
Additionally we examine the newly deposited films for particles using the particle scanner (if available, otherwise we use the Jenatech microscope in darkfield mode) and we monitor the sheet resistance of the Ti/Au or Cr/Au films. | Additionally we examine the newly deposited films for particles using the particle scanner (if available, otherwise we use the Jenatech microscope in darkfield mode) and we monitor the sheet resistance of the Ti/Au or Cr/Au films. | ||
|} | |} | ||