Simple e-beam pattern in this resist has been tested, the results showed on this page. If you have questions to the process or wish to use this e-beam resist, please contact [mailto:lithography@nanolab.dtu.dk lithography] at DTU Nanolab.
Simple e-beam pattern in this resist has been tested, the results showed on this page. If you have questions to the process or wish to use this e-beam resist, please contact [mailto:lithography@nanolab.dtu.dk lithography] at DTU Nanolab.


== Spin Curves ==
== Spin Curves ==
Line 190: Line 186:
|549
|549
|-
|-
|}
|}


<br>
<br>
<br>


== Contrast Curves ==
== Contrast Curve ==


=== CSAR 6200.09 ===
=== CSAR 6200.09 ===


100 nm lines in both ~70 nm and ~188 nm thick CSAR has been developed with AR-600-546 (standard CSAR developer) at room temperature.  
100 nm lines in both ~70 nm and ~188 nm thick CSAR has been developed with AR-600-546 (standard CSAR developer) at room temperature to provide the following contrast curves.


{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;"  style="width: 95%"
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;"  style="width: 95%"
Line 232: Line 223:
|}
|}


[[File:ContrastCurvesCSAR_March2016_log.png|600px]]
{| style="border: none; border-spacing: 0; margin: 1em auto; text-align: center;"
|-
| [[image:ContrastCurvesCSAR_March2016_log.png|600px]]
|-
| colspan="1" style="text-align:center;|
AR-P 6200 contrast curves.
|}


==Dose to size==
Small features need a comparatively higher dose then big features and hence it can be useful to map out the dose and size dependency. Below is a set of cross sectional images of 100, 50 and 20 nm lines written 500, 250 and 180 nm resist at doses from 200 to 600 µC/cm<sup>2</sup>.


{| style="border: none; border-spacing: 0; margin: 1em auto; text-align: center;"
{| style="border: none; border-spacing: 0; margin: 1em auto; text-align: center;"
Line 245: Line 244:
| colspan="1" style="text-align:center;|
| colspan="1" style="text-align:center;|
Cross section SEM images of 500 nm AR-P 6200.09 exposed at 200-600 µC/cm<sup>2</sup>. Top image is 100 nm lines, center image is 50 nm lines, bottom image is 20 nm lines. Au coated for SEM imaging.
Cross section SEM images of 500 nm AR-P 6200.09 exposed at 200-600 µC/cm<sup>2</sup>. Top image is 100 nm lines, center image is 50 nm lines, bottom image is 20 nm lines. Au coated for SEM imaging.
|}
{| style="border: none; border-spacing: 0; margin: 1em auto; text-align: center;"
|-
| [[image:thope240214_lines250_100nm.png|1200px]]
|-
| [[image:thope240214_lines250_50nm.png|1200px]]
|-
| [[image:thope240214_lines250_20nm.png|1200px]]
|-
| colspan="1" style="text-align:center;|
Cross section SEM images of 250 nm AR-P 6200.09 exposed at 200-600 µC/cm<sup>2</sup>. Top image is 100 nm lines, center image is 50 nm lines, bottom image is 20 nm lines. Au coated for SEM imaging.
|}
{| style="border: none; border-spacing: 0; margin: 1em auto; text-align: center;"
|-
| [[image:thope240214_lines180_100_29.png|1200px]]
|-
| [[image:thope240214_lines180_50_31.png|1200px]]
|-
| [[image:thope240214_lines180_20_33.png|1200px]]
|-
| colspan="1" style="text-align:center;|
Cross section SEM images of 180 nm AR-P 6200.09 exposed at 200-600 µC/cm<sup>2</sup>. Top image is 100 nm lines, center image is 50 nm lines, bottom image is 20 nm lines. Au coated for SEM imaging.
|}
|}