Simple e-beam pattern in this resist has been tested, the results showed on this page. If you have questions to the process or wish to use this e-beam resist, please contact [mailto:lithography@nanolab.dtu.dk lithography] at DTU Nanolab. | Simple e-beam pattern in this resist has been tested, the results showed on this page. If you have questions to the process or wish to use this e-beam resist, please contact [mailto:lithography@nanolab.dtu.dk lithography] at DTU Nanolab. | ||
== Spin Curves == | == Spin Curves == | ||
| Line 190: | Line 186: | ||
|549 | |549 | ||
|- | |- | ||
|} | |} | ||
== Contrast | == Contrast Curve == | ||
=== CSAR 6200.09 === | === CSAR 6200.09 === | ||
100 nm lines in both ~70 nm and ~188 nm thick CSAR has been developed with AR-600-546 (standard CSAR developer) at room temperature. | 100 nm lines in both ~70 nm and ~188 nm thick CSAR has been developed with AR-600-546 (standard CSAR developer) at room temperature to provide the following contrast curves. | ||
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;" style="width: 95%" | {|border="1" cellspacing="0" cellpadding="3" style="text-align:left;" style="width: 95%" | ||
| Line 232: | Line 223: | ||
|} | |} | ||
[[ | {| style="border: none; border-spacing: 0; margin: 1em auto; text-align: center;" | ||
|- | |||
| [[image:ContrastCurvesCSAR_March2016_log.png|600px]] | |||
|- | |||
| colspan="1" style="text-align:center;| | |||
AR-P 6200 contrast curves. | |||
|} | |||
==Dose to size== | |||
Small features need a comparatively higher dose then big features and hence it can be useful to map out the dose and size dependency. Below is a set of cross sectional images of 100, 50 and 20 nm lines written 500, 250 and 180 nm resist at doses from 200 to 600 µC/cm<sup>2</sup>. | |||
{| style="border: none; border-spacing: 0; margin: 1em auto; text-align: center;" | {| style="border: none; border-spacing: 0; margin: 1em auto; text-align: center;" | ||
|- | |- | ||
| [[image:thope240214_lines_100_06.png| | | [[image:thope240214_lines_100_06.png|1200px]] | ||
|- | |- | ||
| [[image:thope240214_lines_50_11.png| | | [[image:thope240214_lines_50_11.png|1200px]] | ||
|- | |- | ||
| [[image:thope240214_lines_20_13.png| | | [[image:thope240214_lines_20_13.png|1200px]] | ||
|- | |- | ||
| colspan="1" style="text-align:center;| | | colspan="1" style="text-align:center;| | ||
Cross section SEM images of 500 nm AR-P 6200.09 exposed at 200-600 µC/cm<sup>2</sup>. Top image is 100 nm lines, center image is 50 nm lines, bottom image is 20 nm lines. Au coated for SEM imaging. | Cross section SEM images of 500 nm AR-P 6200.09 exposed at 200-600 µC/cm<sup>2</sup>. Top image is 100 nm lines, center image is 50 nm lines, bottom image is 20 nm lines. Au coated for SEM imaging. | ||
|} | |||
{| style="border: none; border-spacing: 0; margin: 1em auto; text-align: center;" | |||
|- | |||
| [[image:thope240214_lines250_100nm.png|1200px]] | |||
|- | |||
| [[image:thope240214_lines250_50nm.png|1200px]] | |||
|- | |||
| [[image:thope240214_lines250_20nm.png|1200px]] | |||
|- | |||
| colspan="1" style="text-align:center;| | |||
Cross section SEM images of 250 nm AR-P 6200.09 exposed at 200-600 µC/cm<sup>2</sup>. Top image is 100 nm lines, center image is 50 nm lines, bottom image is 20 nm lines. Au coated for SEM imaging. | |||
|} | |||
{| style="border: none; border-spacing: 0; margin: 1em auto; text-align: center;" | |||
|- | |||
| [[image:thope240214_lines180_100_29.png|1200px]] | |||
|- | |||
| [[image:thope240214_lines180_50_31.png|1200px]] | |||
|- | |||
| [[image:thope240214_lines180_20_33.png|1200px]] | |||
|- | |||
| colspan="1" style="text-align:center;| | |||
Cross section SEM images of 180 nm AR-P 6200.09 exposed at 200-600 µC/cm<sup>2</sup>. Top image is 100 nm lines, center image is 50 nm lines, bottom image is 20 nm lines. Au coated for SEM imaging. | |||
|} | |} | ||