Simple e-beam pattern in this resist has been tested, the results showed on this page. If you have questions to the process or wish to use this e-beam resist, please contact [mailto:lithography@nanolab.dtu.dk lithography] at DTU Nanolab.
Simple e-beam pattern in this resist has been tested, the results showed on this page. If you have questions to the process or wish to use this e-beam resist, please contact [mailto:lithography@nanolab.dtu.dk lithography] at DTU Nanolab.


== Spin Curves ==
== Spin Curves ==
Line 190: Line 186:
|549
|549
|-
|-
|}
|}


<br>
<br>
<br>


== Contrast Curves ==
== Contrast Curve ==


=== CSAR 6200.09 ===
=== CSAR 6200.09 ===


100 nm lines in both ~70 nm and ~188 nm thick CSAR has been developed with AR-600-546 (standard CSAR developer) at room temperature.  
100 nm lines in both ~70 nm and ~188 nm thick CSAR has been developed with AR-600-546 (standard CSAR developer) at room temperature to provide the following contrast curves.


{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;"  style="width: 95%"
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;"  style="width: 95%"
Line 232: Line 223:
|}
|}


[[File:ContrastCurvesCSAR_March2016_log.png|600px]]
{| style="border: none; border-spacing: 0; margin: 1em auto; text-align: center;"
|-
| [[image:ContrastCurvesCSAR_March2016_log.png|600px]]
|-
| colspan="1" style="text-align:center;|
AR-P 6200 contrast curves.
|}
 
==Dose to size==
Small features need a comparatively higher dose then big features and hence it can be useful to map out the dose and size dependency. Below is a set of cross sectional images of 100, 50 and 20 nm lines written 500, 250 and 180 nm resist at doses from 200 to 600 µC/cm<sup>2</sup>.
 
{| style="border: none; border-spacing: 0; margin: 1em auto; text-align: center;"
|-
| [[image:thope240214_lines_100_06.png|1200px]]
|-
| [[image:thope240214_lines_50_11.png|1200px]]
|-
| [[image:thope240214_lines_20_13.png|1200px]]
|-
| colspan="1" style="text-align:center;|
Cross section SEM images of 500 nm AR-P 6200.09 exposed at 200-600 µC/cm<sup>2</sup>. Top image is 100 nm lines, center image is 50 nm lines, bottom image is 20 nm lines. Au coated for SEM imaging.
|}


{| style="border: none; border-spacing: 0; margin: 1em auto; text-align: center;"
|-
| [[image:thope240214_lines250_100nm.png|1200px]]
|-
| [[image:thope240214_lines250_50nm.png|1200px]]
|-
| [[image:thope240214_lines250_20nm.png|1200px]]
|-
| colspan="1" style="text-align:center;|
Cross section SEM images of 250 nm AR-P 6200.09 exposed at 200-600 µC/cm<sup>2</sup>. Top image is 100 nm lines, center image is 50 nm lines, bottom image is 20 nm lines. Au coated for SEM imaging.
|}


{| style="border: none; border-spacing: 0; margin: 1em auto; text-align: center;"
{| style="border: none; border-spacing: 0; margin: 1em auto; text-align: center;"
|-
|-
| [[image:thope240214_lines_100_06.png|800px]]
| [[image:thope240214_lines180_100_29.png|1200px]]
|-
| [[image:thope240214_lines180_50_31.png|1200px]]
|-  
|-  
| [[image:thope240214_lines_100_06.png|800px]]
| [[image:thope240214_lines180_20_33.png|1200px]]
|-  
|-  
| colspan="1" style="text-align:center;|
| colspan="1" style="text-align:center;|
.
Cross section SEM images of 180 nm AR-P 6200.09 exposed at 200-600 µC/cm<sup>2</sup>. Top image is 100 nm lines, center image is 50 nm lines, bottom image is 20 nm lines. Au coated for SEM imaging.
|}
|}