Specific Process Knowledge/Lithography/EBeamLithography/AR-P 617: Difference between revisions
Appearance
| (7 intermediate revisions by the same user not shown) | |||
| Line 22: | Line 22: | ||
=Contrast curve= | =Contrast curve= | ||
A contrast curve for AR-P 617.06 is provided below based on exposure at 100 kV for doses from 5 to 120 µC/cm<sup>2</sup>. The dose clear is dependent on softbake temperature, in this case 200C and 180C is used. Process parameters are: | A contrast curve for AR-P 617.06 is provided below based on exposure at 100 kV for doses from 5 to 120 µC/cm<sup>2</sup>. The dose to clear is dependent on softbake temperature, in this case 200C and 180C is used. Process parameters are: | ||
*Date: February 5th 2024 | *Date: February 5th 2024 | ||
| Line 28: | Line 28: | ||
*Substrate: 2" Si | *Substrate: 2" Si | ||
*Acceleration: 1000 RPM/s | *Acceleration: 1000 RPM/s | ||
*Speed: 4000 RPM | |||
*Time: 60 s | *Time: 60 s | ||
*Baking temperature: 200C, 180C and 160C | *Baking temperature: 200C, 180C and 160C | ||
| Line 46: | Line 47: | ||
=Development= | =Development= | ||
AR-P is developed in AR 600-50 and IPA is used to rinse and stop development. As we have no dedicated setup for this it must be done in beakers in the EBL development fumehood in E4. | AR-P 617 is developed in AR 600-50 and IPA is used to rinse and stop development. As we have no dedicated setup for this it must be done in beakers in the EBL development fumehood in E4. | ||
Typical development time is 60-90 seconds and it is recommended to rinse for 30 seconds in IPA. | Typical development time is 60-90 seconds and it is recommended to rinse for 30 seconds in IPA. | ||
| Line 73: | Line 74: | ||
*2nd development | *2nd development | ||
**Manual development in fumehood 10 - AR 600-50 for 90 sec and 30 sec IPA rinse | **Manual development in fumehood 10 - AR 600-50 for 90 sec and 30 sec IPA rinse | ||
The second development can be further extended to promote additional undercut. | |||
{| style="border: none; border-spacing: 0; margin: 1em auto; text-align: center;" | |||
|- | |||
| [[image:ARP617_240212_D1005.png|800px]] | |||
|- | |||
| colspan="1" style="text-align: center;| | |||
Bi-layer resist stack exposed at 400 µC/cm<sup>2</sup>. Au coated for imaging. | |||
|} | |||