Jump to content

Specific Process Knowledge/Lithography/EBeamLithography/AR-P 617: Difference between revisions

Thope (talk | contribs)
Thope (talk | contribs)
 
(10 intermediate revisions by the same user not shown)
Line 22: Line 22:


=Contrast curve=
=Contrast curve=
A contrast curve for AR-P 617.06 is provided below based on exposure at 100 kV for doses from 5 to 120 µC/cm<sup>2</sup>. The dose clear is dependent on softbake temperature, in this case 200C and 180C is used. Process parameters are:
A contrast curve for AR-P 617.06 is provided below based on exposure at 100 kV for doses from 5 to 120 µC/cm<sup>2</sup>. The dose to clear is dependent on softbake temperature, in this case 200C and 180C is used. Process parameters are:


*Date: February 5th 2024
*Date: February 5th 2024
Line 28: Line 28:
*Substrate: 2" Si
*Substrate: 2" Si
*Acceleration: 1000 RPM/s
*Acceleration: 1000 RPM/s
*Speed: 4000 RPM
*Time: 60 s
*Time: 60 s
*Baking temperature: 200C, 180C and 160C
*Baking temperature: 200C, 180C and 160C
Line 46: Line 47:


=Development=
=Development=
AR-P is developed in AR 600-50 and IPA is used to rinse and stop development. As we have no dedicated setup for this it must be done in beakers in the EBL development fumehood in E4.  
AR-P 617 is developed in AR 600-50 and IPA is used to rinse and stop development. As we have no dedicated setup for this it must be done in beakers in the EBL development fumehood in E4.  


Typical development time is 60-90 seconds and it is recommended to rinse for 30 seconds in IPA.
Typical development time is 60-90 seconds and it is recommended to rinse for 30 seconds in IPA.
Line 53: Line 54:


=Dual layer for lift off=
=Dual layer for lift off=
AR-P 617 can be used together with AR-P 6200 (CSAR) for a bi-layer lift-off friendly resist stack, where a slight undercut is made in the bottom layer. AR-P 617 has a higher sensitivity than AR-P 6200 and thus, if AR-P 617 is applied as the bottom layer, the higher sensitivity can lead to an undercut under the AR-P 6200 layer. The example below illustrates the process.
Bi-layer resist stack for lift off process:
*Date: February 12th 2024
*Substrate: 2" Si
*1st layer coating
**Coater: Labspin 2
**RPM: 4000
**Spin time: 60 sec
**Acceleration: 1000 RPM/s
**Soft bake: 200C for 120 sec (setpoint at 222C)
*2nd layer coating
**Coater: Gamma E-beam & UV
**Recipe: 2325-DCH 50mm CSAR 250nm
*Exposure tool: JEOL 9500 - 100 kV @ 29 nA
*1st development
**Developer: EBL Manual
**Recipe: N50 90 sec
*2nd development
**Manual development in fumehood 10 - AR 600-50 for 90 sec and 30 sec IPA rinse
The second development can be further extended to promote additional undercut.
{| style="border: none; border-spacing: 0; margin: 1em auto; text-align: center;"
|-
| [[image:ARP617_240212_D1005.png|800px]]
|-
| colspan="1" style="text-align: center;|
Bi-layer resist stack exposed at 400 µC/cm<sup>2</sup>. Au coated for imaging.
|}