Specific Process Knowledge/Etch/DRIE-Pegasus/Pegasus-4/SiO2 Etch: Difference between revisions
Appearance
No edit summary |
|||
| (5 intermediate revisions by the same user not shown) | |||
| Line 23: | Line 23: | ||
<br clear="all"/> | <br clear="all"/> | ||
===Results with SiO2_res_10 and | ===Results with SiO2_res_10 and with with the electro magnets on=== | ||
[[File:Contour Plot Y31 EM_02_30 white to blue.jpg|400px|thumb|left|Etched with EM:02/30 for 2min, average etch rate: 275 nm/min +- 4.5%. The electro magnets changed the uniformity pattern and made it a bit worse ]] | The SiO2:res_10 recipe was tested with the electromagnets on but it seems to no no good for the results.[[File:Contour Plot Y31 EM_02_30 white to blue.jpg|400px|thumb|left|Etched with EM:02/30 for 2min, average etch rate: 275 nm/min +- 4.5%. The electro magnets changed the uniformity pattern and made it a bit worse ]] | ||
<br clear="all"/> | <br clear="all"/> | ||
| Line 36: | Line 36: | ||
</gallery> | </gallery> | ||
Using the electromagnetic coil on the recipe SiO2_res_10 gave higher etch rate on this chip | Using the electromagnetic coil on the recipe SiO2_res_10 gave higher etch rate on this chip, which is positioned in the center of a 6" wafer. The Etch profile is more angled. | ||
*Removing the H2 from the recipe to get less redeposition at lower platen power (200W), EM:02/30A. Se result below. This gave significantly lower etch rate and no etching in the smallest openings. | |||
<gallery caption="Recipe name: SiO2_res, Recipe no. 10+EM+edit coils: C09975 coil_2500W, platen:200W, EM:02/30A, Pressure:8.8mTorr, C4F8:25.6sccm, He:448.7sccm, H2:0sccm, 3:56 min " perrow="5"> | |||
File:C09975_00.jpg | |||
File:C09975_02.jpg | |||
File:C09975_03.jpg | |||
File:C09975_04.jpg | |||
File:C09975_05.jpg | |||
</gallery> | </gallery> | ||
< | <br clear="all"/> | ||
==SiO2 etch with Cr mask== | ==SiO2 etch with Cr mask== | ||
| Line 86: | Line 58: | ||
===SiO2 etch with Cr mask 100 nm and with 500 nm for the resist for the Cr etch=== | ===SiO2 etch with Cr mask 100 nm and with 500 nm for the resist for the Cr etch=== | ||
Barc etch and Cr etch were done in ICP metal using end point detection. The sample was a full 6" wafer | Barc etch and Cr etch were done in ICP metal using end point detection. The sample was a full 6" wafer | ||
<gallery caption="SiO2_res_10 2x5:00 min with 3 min TDESC clean in between 100 nm Cr mask | <gallery caption="SiO2_res_10 2x5:00 min with 3 min TDESC clean in between 100 nm Cr mask, with 500 nm resist" widths="200px" heights="200px" perrow="6"> | ||
File:C041630_center_07.jpg | File:C041630_center_07.jpg | ||
File:C041630_center_08.jpg | File:C041630_center_08.jpg | ||
| Line 103: | Line 75: | ||
<gallery caption="SiO2_res_10 5:00 min 100 nm Cr mask | <gallery caption="SiO2_res_10 5:00 min 100 nm Cr mask, with 500 nm resist, resist/Cr stripped after etch in plasma asher 35min" widths="250px" heights="250px" perrow="4"> | ||
File:S0411376_profile_20.jpg| 200nm/400nm | File:S0411376_profile_20.jpg| 200nm/400nm | ||
File:S0411376_profile_13.jpg|250nm/500nm | File:S0411376_profile_13.jpg|250nm/500nm | ||
| Line 112: | Line 84: | ||
</gallery> | </gallery> | ||
===Testing with electromagnetic coils /Cr mask=== | ===Testing with electromagnetic coils /Cr mask=== | ||
| Line 174: | Line 145: | ||
File:C09721_center_21.jpg | File:C09721_center_21.jpg | ||
File:C09721_center_22.jpg | File:C09721_center_22.jpg | ||
</gallery> | |||
==SiO2 Etch using aSi as masking material== | |||
{{CC-bghe2}} <br> | |||
I was starting up development of SiO2 etch using aSi as masking material. This is on pause because the results did not look promishing on high aspect ratio structures wit DUV pattern due to large faceting on the aSi mask. I turned to Cr mask instead <br> | |||
The samples I use are: | |||
*6" Si afters with oxide (2µm), | |||
*aSi (~300nm), | |||
*Neg. DUV reist (~60nm barc, ~350 nm resist) | |||
*Reticle: Danchip/Triple-D | |||
*Dose 230 J/m2 | |||
First I need to make sure that the resist work for pattering the aSi layer is good. If the resist is not good the final etch will also not be good. | |||
===DUV optimization=== | |||
Dose test with the doses (J/m2): 200, 210, 220, 230, 240, 250, 270, 280 | |||
The aim was to get good line for 400nm pitch/200nm lines | |||
<gallery caption="400nm pitch 200 nm lines" perrow="5" widths="200px" heights="150px"> | |||
Image:dose200_no2_22.jpg |200 J/m2 400nm/268nm | |||
Image:dose210_no2_15.jpg |210 J/m2 400nm/239nm | |||
Image:dose220_no2_13.jpg |220 J/m2 400nm/208nm | |||
Image:dose230_no2_11.jpg |230 J/m2 400nm/209nm | |||
Image:dose240_no2_05.jpg |240 J/m2 400nm/215nm | |||
Image:dose250_no2_11.jpg |250 J/m2 400nm/207nm | |||
Image:dose260_no2_18.jpg |260 J/m2 400nm/188nm | |||
Image:dose270_no2_24.jpg |270 J/m2 400nm/155nm | |||
Image:dose280_no1_15.jpg |280 J/m2 400nm/0nm | |||
</gallery> | |||
<gallery caption="1000nm pitch 500 nm lines" perrow="3" widths="200px" heights="150px"> | |||
Image:dose210_no2_17.jpg |210 J/m2 1000nm/581nm | |||
Image:dose230_no2_12.jpg |230 J/m2 1000nm/517nm | |||
Image:dose240_no2_03.jpg |240 J/m2 1000nm/518nm | |||
Image:dose250_no2_09.jpg |250 J/m2 1000nm/510nm | |||
Image:dose260_no2_15.jpg |260 J/m2 1000nm/493nm | |||
Image:dose270_no2_22.jpg |270 J/m2 1000nm/494nm | |||
</gallery> | </gallery> | ||