Specific Process Knowledge/Thin film deposition/Deposition of Nickel: Difference between revisions
| (12 intermediate revisions by 2 users not shown) | |||
| Line 1: | Line 1: | ||
{{cc-nanolab}} | |||
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Nickel click here]''' | '''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Nickel click here]''' | ||
== Nickel deposition == | == Nickel deposition == | ||
| Line 10: | Line 9: | ||
Some process information is available here for e-beam evaporated films: | Some process information is available here for e-beam evaporated films: | ||
<!--*[[/Electroplating of nickel|Electroplating of nickel]]--> | <!--*[[/Electroplating of nickel|Electroplating of nickel]]--> | ||
*[[/Stress Wordentec Ni films|Stress in | *[[/Stress Wordentec Ni films|Stress in e-beam evaporated Ni films: study here]] ''(from the now decommissioned Wordentec deposition tool - basic trends in results should be transferable to other e-beam evaporators).'' | ||
In the chart below you can compare the different deposition equipment: | In the chart below you can compare the different deposition equipment: | ||
| Line 18: | Line 17: | ||
! | ! | ||
! E-beam evaporation ([[Specific Process Knowledge/Thin film deposition/Temescal|E-beam evaporator (Temescal)]] and [[Specific Process Knowledge/Thin film deposition/10-pocket e-beam evaporator|E-beam evaporator (10-pockets)]]) | ! E-beam evaporation ([[Specific Process Knowledge/Thin film deposition/Temescal|E-beam evaporator (Temescal)]] and [[Specific Process Knowledge/Thin film deposition/10-pocket e-beam evaporator|E-beam evaporator (10-pockets)]]) | ||
! Sputter deposition ([[Specific Process Knowledge/Thin film deposition/Lesker|Lesker]]) | ! Sputter deposition ([[Specific Process Knowledge/Thin film deposition/Lesker|Lesker]]) | ||
! Sputter deposition ([[Specific Process Knowledge/Thin film deposition/Cluster-based multi-chamber high vacuum sputtering deposition system|Sputter-system Metal-Oxide (PC1) and Sputter-system Metal-Nitride (PC3)]]) | ! Sputter deposition ([[Specific Process Knowledge/Thin film deposition/Cluster-based multi-chamber high vacuum sputtering deposition system|Sputter-system Metal-Oxide (PC1) and Sputter-system Metal-Nitride (PC3)]]) | ||
| Line 26: | Line 24: | ||
! General description | ! General description | ||
|E-beam deposition of Nickel | |E-beam deposition of Nickel | ||
|Sputter deposition of Nickel | |Sputter deposition of Nickel | ||
| Line 37: | Line 34: | ||
|Ar ion etch (only in E-beam evaporator Temescal) | |Ar ion etch (only in E-beam evaporator Temescal) | ||
| | | | ||
|RF Ar clean | |RF Ar clean | ||
|- | |- | ||
| Line 44: | Line 40: | ||
! Layer thickness | ! Layer thickness | ||
|10 Å to 1 µm * | |10 Å to 1 µm * | ||
|10 Å to | |10 Å to 500 nm ** | ||
|10 Å to 500 nm ** | |||
|10 Å to | |||
|- | |- | ||
|-style="background:LightGrey; color:black" | |-style="background:LightGrey; color:black" | ||
! Deposition rate | ! Deposition rate | ||
|1-10 Å/s | |1-10 Å/s | ||
|Depends on process parameters, about 1 Å/s | |Depends on process parameters, about 1 Å/s | ||
| Line 63: | Line 57: | ||
*Up to 3x8" wafers (ask for holder) | *Up to 3x8" wafers (ask for holder) | ||
*Many smaller pieces | *Many smaller pieces | ||
| | | | ||
* Pieces or | * Pieces or | ||
| Line 81: | Line 71: | ||
| | | | ||
*Almost any that does not degas at your intended substrate temperature. See also the [ | *Almost any that does not degas at your intended substrate temperature. See also the [https://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=429 cross-contamination sheet] | ||
| | | | ||
Almost any that | * Almost any that do not degas. See also the [https://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=244 cross-contamination sheet] | ||
| | | | ||
*Almost any that does not degas at your intended substrate temperature. See cross contamination sheets for [https://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=441 PC1] and [https://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=442 PC3] | |||
*Almost any that does not degas at your intended substrate temperature. See cross contamination sheets for [ | |||
|- | |- | ||
| Line 94: | Line 82: | ||
! Comment | ! Comment | ||
| | | | ||
| | | | ||
*May use high-strength magnet for deposition. | *May use high-strength magnet for deposition. | ||
| Line 110: | Line 96: | ||
==Quality control of e-beam evaporated Ni films== | ==Quality control of e-beam evaporated Ni films== | ||
{| border="1" cellspacing="2" cellpadding="2" colspan="3" | {| border="1" cellspacing="2" cellpadding="2" colspan="3" | ||
|bgcolor="#98FB98" |'''Quality control (QC) for | |bgcolor="#98FB98" |'''Quality control (QC) for the E-beam Evaporator (Temescal) and the E-beam Evaporator (10-pockets)''' | ||
|- | |- | ||
| | | | ||
Nickel deposition is tested occasionally, around 1 | Nickel deposition is tested occasionally, around 1 time per year in each machine. You are welcome to contact staff to request an extra test of the material. | ||
'''LabManager links to procedures and data''' (require login): | |||
*[http://labmanager.dtu.dk/d4Show.php?id=5862&mach=429 QC procedure for the E-beam Evaporator (Temescal)]<br> | |||
*[https://labmanager.dtu.dk/view_binary.php?type=data&mach=429 The newest QC data for the E-beam Evaporator (Temescal)]<br> | |||
*[http://labmanager.dtu.dk/d4Show.php?id=5862&mach=511 QC procedure for the E-beam Evaporator (10-pockets)]<br> | |||
*[https://labmanager.dtu.dk/view_binary.php?type=data&mach=511 The newest QC data for the E-beam Evaporator (10-pockets)]<br> | |||
{| {{table}} | {| {{table}} | ||
| align=" | | align="left" valign="top"| | ||
{| border=" | {| border="2" cellspacing="1" cellpadding="2" align="left" style="width:400px" | ||
! QC Recipe: | ! QC Recipe: | ||
! Standard recipes/Ni | ! Standard recipes/Ni | ||
|- | |- | ||
|Deposition rate | |Deposition rate | ||
| | |2 Å/s | ||
|- | |- | ||
|Thickness | |Thickness | ||
| Line 179: | Line 127: | ||
|- | |- | ||
|} | |} | ||
| align=" | |- | ||
{| border="2" cellspacing="1" cellpadding="2" align=" | |} | ||
{| {{table}} | |||
| align="left" valign="top"| | |||
{| border="2" cellspacing="1" cellpadding="2" align="left" style="width:400px" | |||
!QC limits | !QC limits | ||
! | !Both E-beam Evaporators | ||
|- | |- | ||
|Deposition rate deviation | |Deposition rate deviation | ||
| Line 196: | Line 149: | ||
|- | |- | ||
|} | |} | ||
Thickness is measured in 5 points with a stylus profiler. <br> | |||
Thickness is measured in 5 points with a stylus profiler (usually DektakXT). <br> | |||
|} | |} | ||
Latest revision as of 23:56, 7 July 2025
The content on this page, including all images and pictures, was created by DTU Nanolab staff, unless otherwise stated.
Feedback to this page: click here
Nickel deposition
Nickel can be deposited by e-beam evaporation or sputtering at DTU Nanolab. For electroplating you will have to contact other institutes at DTU, e.g., DTU Mechanical Engineering.
Some process information is available here for e-beam evaporated films:
- Stress in e-beam evaporated Ni films: study here (from the now decommissioned Wordentec deposition tool - basic trends in results should be transferable to other e-beam evaporators).
In the chart below you can compare the different deposition equipment:
| E-beam evaporation (E-beam evaporator (Temescal) and E-beam evaporator (10-pockets)) | Sputter deposition (Lesker) | Sputter deposition (Sputter-system Metal-Oxide (PC1) and Sputter-system Metal-Nitride (PC3)) | |
|---|---|---|---|
| General description | E-beam deposition of Nickel | Sputter deposition of Nickel | Sputter deposition of Nickel |
| Pre-clean | Ar ion etch (only in E-beam evaporator Temescal) | RF Ar clean | |
| Layer thickness | 10 Å to 1 µm * | 10 Å to 500 nm ** | 10 Å to 500 nm ** |
| Deposition rate | 1-10 Å/s | Depends on process parameters, about 1 Å/s | Depends on process parameters, at least ~ 4 Å/s, see conditions here |
| Batch size |
|
|
|
| Allowed materials |
|
|
|
| Comment |
|
|
* To deposit a cumulative thickness above 600 nm permission is required from metal@nanolab.dtu.dk to ensure enough material is present in the machine
** To deposit a cumulative thickness above 200 nm permission is required from metal@nanolab.dtu.dk to ensure enough material is present in the machine
Quality control of e-beam evaporated Ni films
| Quality control (QC) for the E-beam Evaporator (Temescal) and the E-beam Evaporator (10-pockets) | ||||||||||||||||||
|
Nickel deposition is tested occasionally, around 1 time per year in each machine. You are welcome to contact staff to request an extra test of the material. LabManager links to procedures and data (require login):
Thickness is measured in 5 points with a stylus profiler (usually DektakXT). |