This page presents the results of Scandium Nitride deposition using <b>RF</b> Reactive Sputtering in Sputter-System Metal-Nitride (PC3) commonly known as "Cluster Lesker". The deposition target is 4" <b>Sc</b> (0. | This page presents the results of Scandium Nitride deposition using <b>RF</b> Reactive Sputtering in Sputter-System Metal-Nitride (PC3) commonly known as "Cluster Lesker". The deposition target is 4" <b>Sc</b> (0.250" Indium bonded with indium to 3mm Cu plate). Source #1 was used. Materials (ScN) from this source can either be deposited with RF or p-DC sputtering although only RF mode has been tested so far. | ||
| Line 40: | Line 40: | ||
Samples: 6" Si. | Samples: 6" Si without native oxide (HF-treated). | ||
<gallery caption="The photography of Sc target mounted in 4” magnetron (PC3 Src1). "widths="400px" heights="500px" perrow="2"> | <gallery caption="The photography of Sc target mounted in 4” magnetron (PC3 Src1). "widths="400px" heights="500px" perrow="2"> | ||
| Line 141: | Line 141: | ||
==X-ray Reflectivity (XRR)== | ==X-ray Reflectivity (XRR)== | ||
[[Specific Process Knowledge/Characterization/XRD/XRD_SmartLab|X-ray Reflectivity]] analysis of ScN samples have been performed to investigate the thicknesses, roughness, and density profiles. | |||
The scans has been obtained using Rigaku XRD SmartLab equipment. The voltage and current settings for the Cu X-ray tube were standard 40kV and 30mA. The incident optics contained a IPS (incident parallel slit) adaptor with 5 ° Soller slit. Other slits: IS=0.05mm RS1=0.05mm and RS2=0.075mm. Step size: 0.01 and measurement time - 5s for each point. Fitting procesure was performed using commercial GlobalFit software assuming the model based on Si substrate followed by Sc-Si transition layer for better fit, followed by the main ScN film with thin oxides and moisture surfaces. The results are summarized in a tables below. | |||
<gallery caption="X-ray reflectivity scans of ScN thin films (PC3 Src1). " widths="450px" heights="400px" perrow="3"> | <gallery caption="X-ray reflectivity scans of ScN thin films (PC3 Src1). " widths="450px" heights="400px" perrow="3"> | ||
image:eves_XRR_ScN_3mTorr_1000s_200W_PC3_Src1_RF_ext_20231013.png|ScN thin film XRR. Power: 200W, Deposition time: 1000s, Pressure 3 mTorr. PC Gun Z-shift Position: Extended (95.20 mm). | image:eves_XRR_ScN_3mTorr_1000s_200W_PC3_Src1_RF_ext_20231013.png|ScN thin film XRR. Power: 200W, Deposition time: 1000s, Pressure 3 mTorr. PC Gun Z-shift Position: Extended (95.20 mm). | ||
image:eves_XRR_ScN_3mTorr_1000s_150W_PC3_Src1_RF_ext_20231013.png|ScN thin film XRR. Power: | image:eves_XRR_ScN_3mTorr_1000s_150W_PC3_Src1_RF_ext_20231013.png|ScN thin film XRR. Power: 150W, Deposition time: 1000s, Pressure 3 mTorr. PC Gun Z-shift Position: Extended (95.20 mm). | ||
image:eves_XRR_ScN_3mTorr_1000s_100W_PC3_Src1_RF_ext_20231013.png|ScN thin film XRR. Power: | image:eves_XRR_ScN_3mTorr_1000s_100W_PC3_Src1_RF_ext_20231013.png|ScN thin film XRR. Power: 100W, Deposition time: 1000s, Pressure 3 mTorr. PC Gun Z-shift Position: Extended (95.20 mm). | ||
</gallery> | </gallery> | ||
<gallery caption="X-ray reflectivity scans of ScN thin films (PC3 Src1). " widths="450px" heights="400px" perrow="3"> | <gallery caption="X-ray reflectivity scans of ScN thin films (PC3 Src1). " widths="450px" heights="400px" perrow="3"> | ||
image:eves_XRR_ScN_3mTorr_1000s_200W_PC3_Src1_RF_home_20231013.png|ScN thin film XRR. Power: 200W, Deposition time: 1000s, Pressure 3 mTorr. PC Gun Z-shift Position: | image:eves_XRR_ScN_3mTorr_1000s_200W_PC3_Src1_RF_home_20231013.png|ScN thin film XRR. Power: 200W, Deposition time: 1000s, Pressure 3 mTorr. PC Gun Z-shift Position: Home (00.00 mm). | ||
image:eves_XRR_ScN_3mTorr_1000s_150W_PC3_Src1_RF_home_20231013.png|ScN thin film XRR. Power: | image:eves_XRR_ScN_3mTorr_1000s_150W_PC3_Src1_RF_home_20231013.png|ScN thin film XRR. Power: 150W, Deposition time: 1000s, Pressure 3 mTorr. PC Gun Z-shift Position: Home (00.00 mm). | ||
image:eves_XRR_ScN_3mTorr_1000s_100W_PC3_Src1_RF_home_20231013.png|ScN thin film XRR. Power: | image:eves_XRR_ScN_3mTorr_1000s_100W_PC3_Src1_RF_home_20231013.png|ScN thin film XRR. Power: 100W, Deposition time: 1000s, Pressure 3 mTorr. PC Gun Z-shift Position: Home (00.00 mm). | ||
</gallery> | </gallery> | ||
| Line 533: | Line 539: | ||
</gallery> | </gallery> | ||
==Scanning Electron | ==Scanning Electron Microscopy== | ||
The images below present SEM images of the ScN layers from the top and tilted view. | The images below present [[Specific Process Knowledge/Characterization/SEM: Scanning Electron Microscopy |Scanning Electron Microscopy (SEM)]] images of the ScN layers from the top and tilted view. | ||
<gallery caption="Scanning Electron Microscopy." widths="480px" heights="400px" perrow="3"> | <gallery caption="Scanning Electron Microscopy." widths="480px" heights="400px" perrow="3"> | ||
image:eves_SEM_ScN_3mTorr_1000s_200W_PC3_Src1_RF_ext_image1_20231013.png| <b><span style="color: red">ScN</span></b> layer deposited at 200 W RF power, 3mTorr, and 1000s. Gun Z-shift position is "Extended". Top view. | image:eves_SEM_ScN_3mTorr_1000s_200W_PC3_Src1_RF_ext_image1_20231013.png| <b><span style="color: red">ScN</span></b> layer deposited at 200 W RF power, 3mTorr, and 1000s. Gun Z-shift position is "Extended". Top view. | ||
image:eves_SEM_ScN_3mTorr_1000s_200W_PC3_Src1_RF_ext_image2_20231013.png| <b><span style="color: red">ScN</span></b> layer deposited at 200 W RF power, 3mTorr, and 1000s. Gun Z-shift position is "Extended". Tilted view. | image:eves_SEM_ScN_3mTorr_1000s_200W_PC3_Src1_RF_ext_image2_20231013.png| <b><span style="color: red">ScN</span></b> layer deposited at 200 W RF power, 3mTorr, and 1000s. Gun Z-shift position is "Extended". Tilted view. | ||
image:eves_SEM_ScN_3mTorr_1000s_200W_PC3_Src1_RF_ext_image3_20231013.png| <b><span style="color: red">ScN</span></b> layer deposited at 200 W RF power, 3mTorr, and 1000s. Gun Z-shift position is "Extended". Tilted view | image:eves_SEM_ScN_3mTorr_1000s_200W_PC3_Src1_RF_ext_image3_20231013.png| <b><span style="color: red">ScN</span></b> layer deposited at 200 W RF power, 3mTorr, and 1000s. Gun Z-shift position is "Extended". Tilted view | ||
</gallery> | </gallery> | ||