Jump to content

Specific Process Knowledge/Thin film deposition/Deposition of Scandium Nitride/ScN Reactive Sputtering in Cluster Lesker PC3: Difference between revisions

From LabAdviser
Eves (talk | contribs)
Eves (talk | contribs)
No edit summary
 
(19 intermediate revisions by the same user not shown)
Line 8: Line 8:




This page presents the results of Scandium Nitride deposition using <b>RF</b> Reactive Sputtering in Sputter-System Metal-Nitride (PC3) commonly known as "Cluster Lesker". The deposition target is 4" <b>Sc</b> (0.25" Indium bonded to Cu plate). Source #1 was used. Materials (ScN) from this source can either be deposited with RF or p-DC sputtering although only RF mode has been tested so far.  
This page presents the results of Scandium Nitride deposition using <b>RF</b> Reactive Sputtering in Sputter-System Metal-Nitride (PC3) commonly known as "Cluster Lesker". The deposition target is 4" <b>Sc</b> (0.250" Indium bonded with indium to 3mm Cu plate). Source #1 was used. Materials (ScN) from this source can either be deposited with RF or p-DC sputtering although only RF mode has been tested so far.  




Line 25: Line 25:
The RF ScN process recipe in a Sputter-System Metal-Nitride(PC3) is following:
The RF ScN process recipe in a Sputter-System Metal-Nitride(PC3) is following:


  * Recipe Name:  <b>MD PC3_Src1 - RF_Downstream with Reactive O2</b>
  * Recipe Name:  <b>MD PC3_Src1 - RF_Downstream with Reactive N2</b>


* PC Gun Z-shift Position: Home (00.00 mm) and Extended (95.20 mm)
* PC Gun Z-shift Position: Home (00.00 mm) and Extended (95.20 mm)
Line 35: Line 35:
* Ar flow: <b>40 sccm</b>
* Ar flow: <b>40 sccm</b>
* N<sub>2</sub> flow: <b>18 sccm</b>
* N<sub>2</sub> flow: <b>18 sccm</b>
* Deposition time: <b>variable</b>
* Deposition time: <b>1000 s</b>
* Deposition temperature: <b>400 &deg;C</b>
* Deposition temperature: <b>400 &deg;C</b>
* Pre-sputtering time : 300s (better to give longer time to sputter away the native oxide, especially on a recently installed target)
* Pre-sputtering time : 300s (better to give longer time to sputter away the native oxide, especially on a recently installed target)




Samples: 6" Si.
Samples: 6" Si without native oxide (HF-treated).


<gallery caption="The photography of Sc target mounted in 4” magnetron (PC3 Src1). "widths="400px" heights="500px" perrow="2">
<gallery caption="The photography of Sc target mounted in 4” magnetron (PC3 Src1). "widths="400px" heights="500px" perrow="2">
Line 141: Line 141:


==X-ray Reflectivity (XRR)==
==X-ray Reflectivity (XRR)==
[[Specific Process Knowledge/Characterization/XRD/XRD_SmartLab|X-ray Reflectivity]] analysis of ScN samples have been performed to investigate the thicknesses, roughness, and density profiles.
The scans has been obtained using Rigaku XRD SmartLab equipment. The voltage and current settings for the Cu X-ray tube were standard  40kV and 30mA. The incident optics contained a IPS (incident parallel slit) adaptor with 5 &deg; Soller slit. Other slits: IS=0.05mm RS1=0.05mm and RS2=0.075mm. Step size: 0.01 and measurement time - 5s for each point. Fitting procesure was performed using commercial GlobalFit software assuming the model based on Si  substrate  followed by Sc-Si transition layer for better fit, followed by the main ScN film with thin oxides and moisture surfaces. The results are summarized in a tables below.


<gallery caption="X-ray reflectivity scans of ScN thin films (PC3 Src1). " widths="450px" heights="400px" perrow="3">
<gallery caption="X-ray reflectivity scans of ScN thin films (PC3 Src1). " widths="450px" heights="400px" perrow="3">
image:eves_XRR_ScN_3mTorr_1000s_200W_PC3_Src1_RF_ext_20231013.png|ScN thin film XRR. Power: 200W, Deposition time: 1000s, Pressure 3 mTorr. PC Gun Z-shift Position: Extended (95.20 mm).
image:eves_XRR_ScN_3mTorr_1000s_200W_PC3_Src1_RF_ext_20231013.png|ScN thin film XRR. Power: 200W, Deposition time: 1000s, Pressure 3 mTorr. PC Gun Z-shift Position: Extended (95.20 mm).
image:eves_XRR_ScN_3mTorr_1000s_150W_PC3_Src1_RF_ext_20231013.png|ScN thin film XRR. Power: 200W, Deposition time: 1000s, Pressure 3 mTorr. PC Gun Z-shift Position: Extended (95.20 mm).
image:eves_XRR_ScN_3mTorr_1000s_150W_PC3_Src1_RF_ext_20231013.png|ScN thin film XRR. Power: 150W, Deposition time: 1000s, Pressure 3 mTorr. PC Gun Z-shift Position: Extended (95.20 mm).
image:eves_XRR_ScN_3mTorr_1000s_100W_PC3_Src1_RF_ext_20231013.png|ScN thin film XRR. Power: 200W, Deposition time: 1000s, Pressure 3 mTorr. PC Gun Z-shift Position: Extended (95.20 mm).
image:eves_XRR_ScN_3mTorr_1000s_100W_PC3_Src1_RF_ext_20231013.png|ScN thin film XRR. Power: 100W, Deposition time: 1000s, Pressure 3 mTorr. PC Gun Z-shift Position: Extended (95.20 mm).
</gallery>
</gallery>


<gallery caption="X-ray reflectivity scans of ScN thin films (PC3 Src1). " widths="450px" heights="400px" perrow="3">
<gallery caption="X-ray reflectivity scans of ScN thin films (PC3 Src1). " widths="450px" heights="400px" perrow="3">
image:eves_XRR_ScN_3mTorr_1000s_200W_PC3_Src1_RF_home_20231013.png|ScN thin film XRR. Power: 200W, Deposition time: 1000s, Pressure 3 mTorr. PC Gun Z-shift Position: Extended (00.00 mm).
image:eves_XRR_ScN_3mTorr_1000s_200W_PC3_Src1_RF_home_20231013.png|ScN thin film XRR. Power: 200W, Deposition time: 1000s, Pressure 3 mTorr. PC Gun Z-shift Position: Home (00.00 mm).
image:eves_XRR_ScN_3mTorr_1000s_150W_PC3_Src1_RF_home_20231013.png|ScN thin film XRR. Power: 200W, Deposition time: 1000s, Pressure 3 mTorr. PC Gun Z-shift Position: Extended (00.00 mm).
image:eves_XRR_ScN_3mTorr_1000s_150W_PC3_Src1_RF_home_20231013.png|ScN thin film XRR. Power: 150W, Deposition time: 1000s, Pressure 3 mTorr. PC Gun Z-shift Position: Home (00.00 mm).
image:eves_XRR_ScN_3mTorr_1000s_100W_PC3_Src1_RF_home_20231013.png|ScN thin film XRR. Power: 200W, Deposition time: 1000s, Pressure 3 mTorr. PC Gun Z-shift Position: Extended (00.00 mm).
image:eves_XRR_ScN_3mTorr_1000s_100W_PC3_Src1_RF_home_20231013.png|ScN thin film XRR. Power: 100W, Deposition time: 1000s, Pressure 3 mTorr. PC Gun Z-shift Position: Home (00.00 mm).
</gallery>
</gallery>


Line 210: Line 216:


|-  
|-  
|<b>150W, 3mTorr, 1050s</b>   
|<b>150W, 3mTorr, 1000s</b>   
|0.63
|0.63
|0.67
|0.67
Line 306: Line 312:


|-  
|-  
|<b>150W, 3mTorr, 1050s</b>   
|<b>150W, 3mTorr, 1000s</b>   
|1.29
|1.29
|1.17
|1.17
Line 498: Line 504:


<br clear="all" />
<br clear="all" />


==X-ray Photoelectron Spectroscopy==
==X-ray Photoelectron Spectroscopy==


X-ray Photoelectron Spectroscopy (XPS) was employed to investigate the chemical composition of deposited scandium nitride (ScN) thin films using the XPS K-alpha instrument. The analysis was conducted in a 'depth profile' mode, where the film was incrementally etched, and the composition was measured layer by layer. Multiple scans were performed, including survey scans and scans for specific elements like O1s, N1s, Sc2p, Sc3s, and C1s, to gather comprehensive chemical information.
[[Specific Process Knowledge/Characterization/XPS|X-ray Photo Electron Spectroscopy (XPS)]] was employed to investigate the chemical composition of deposited scandium nitride (ScN) thin films using the [[Specific Process Knowledge/Characterization/XPS/K-Alpha|XPS K-Alpha]] instrument. The analysis was conducted in a 'depth profile' mode, where the film was incrementally etched, and the composition was measured layer by layer. Multiple scans were performed, including survey scans and scans for specific elements like O1s, N1s, Sc2p, Sc3s, and C1s, to gather comprehensive chemical information.


Interpreting the stoichiometry of the ScN film is challenging due to the overlap between the N1s peak and the Sc2p peak. Additionally, while scandium has various interesting electronic states that can be measured and utilized in calculations (such as Sc3s), there is only one electronic state for nitrogen, N1s, which requires careful deconvolution from the Sc2p peak.
Interpreting the stoichiometry of the ScN film is challenging due to the overlap between the N1s peak and the Sc2p peak. Additionally, while scandium has various interesting electronic states that can be measured and utilized in calculations (such as Sc3s), there is only one electronic state for nitrogen, N1s, which requires careful deconvolution from the Sc2p peak.
Line 508: Line 513:
The ScN sample used for XPS analysis was deposited at the PC Gun Z-shift Extended position (95.20mm) under the following conditions: 400&deg;C, Ar/N 40/18 sccm, 200W power, 3mTorr pressure, and a deposition time of 1000 seconds.
The ScN sample used for XPS analysis was deposited at the PC Gun Z-shift Extended position (95.20mm) under the following conditions: 400&deg;C, Ar/N 40/18 sccm, 200W power, 3mTorr pressure, and a deposition time of 1000 seconds.


<gallery caption="X-ray reflectivity scans of Sc thin films (PC3 Src1). " widths="450px" heights="400px" perrow="3">
Estimated stoichiometry is following: N=37.73%, Sc=48.11%, O=13.89%.
image:eves_XPS_ScN_PC3_Src1_RF_Survej_2031019.png|Sc thin film XRR. Power: 200W, Deposition time: 500s, Pressure 3 mTorr. PC Gun Z-shift Position: Extended (95.20 mm).
 
image:eves_XPS_ScN_PC3_Src1_RF_Sc_3s_fit_2031019.png|Sc thin film XRR. Power: 150W, Deposition time: 750s, Pressure 3 mTorr. PC Gun Z-shift Position: Home (00.00 mm).
The Sc target used in the experiment was new, and due to its susceptibility to oxidation, there is a possibility of a pronounced level of Scandium oxynitride formation. We believe that more extensive usage of the target will remove the oxidized top layer. Additionally, it is necessary to perform preconditioning (pre-sputtering) of the target before using it in applications. This pre-sputtering process will help minimize the oxygen level in the resulting film.
image:eves_XPS_ScN_PC3_Src1_RF_O_s1_fit_2031019.png|Sc thin film XRR. Power: 200W, Deposition time: 500s, Pressure 3 mTorr. PC Gun Z-shift Position: Home (00.00 mm).
 
image:eves_XPS_ScN_PC3_Src1_RF_Sc2p_and_N1s_fit_2031019.png|Sc thin film XRR. Power: 150W, Deposition time: 750s, Pressure 3 mTorr. PC Gun Z-shift Position: Home (00.00 mm).
<gallery caption="X-ray Photoelectron Spectroscopy of ScN thin films (PC3 Src1). High resolution scans fitted with Lorentz-Gaussian functions." widths="450px" heights="400px" perrow="3">
image:eves_XPS_ScN_PC3_Src1_RF_N_s1_fit_2031019_new.png|Sc thin film XRR. Power: 150W, Deposition time: 750s, Pressure 3 mTorr. PC Gun Z-shift Position: Home (00.00 mm).
image:eves_XPS_ScN_PC3_Src1_RF_Survej_2031019.png|Survey spectrum of ScN thin film. The films has been etched for 160s wiht Ar<sup>+</sup> ions at low current and 1000eV energy.
image:eves_XPS_ScN_PC3_Src1_RF_Sc_3s_fit_2031019.png|<b>Sc 3s</b> signal with fitted functions. Useful for stoichiometry calculation, due to the profile simplicity. The film has been etched for 160s wiht Ar<sup>+</sup> ions at low current and 1000eV energy before the scan.
image:eves_XPS_ScN_PC3_Src1_RF_O_s1_fit_2031019.png|<b>O 1s</b> signal with fitted functions. The film has been etched for 160s wiht Ar<sup>+</sup> ions at low current and 1000eV energy before the scan.
image:eves_XPS_ScN_PC3_Src1_RF_Sc2p_and_N1s_fit_2031019.png|<b>Sc 2p</b> and <b>N 1s</b> (in yellow) signals with fitted functions. Less useful for stoichiometry calculation, due to the profile complexity. N1s is dangerously close to Sc 2p, and need to be deconvolved. The film has been etched for 160s wiht Ar<sup>+</sup> ions at low current and 1000eV energy before the scan.
image:eves_XPS_ScN_PC3_Src1_RF_N_s1_fit_2031019_new.png|<b>N 1s</b> (in yellow) signal with fitted functions, where <b>Sc 2p</b> is also present (grey fitted area). Difficult for stoichiometry calculation, due to the profile complexity. N1s is dangerously close to Sc 2p, and need to be deconvolved. However, there are no other electronic states of nitrogen that can be used in XPS, so the deconvolution approach is the only option. The film has been etched for 160s with Ar<sup>+</sup> ions at low current and 1000eV energy before the scan.
</gallery>
</gallery>


<gallery caption="X-ray reflectivity scans of Sc thin films (PC3 Src1). " widths="450px" heights="400px" perrow="3">
<gallery caption="X-ray Photoelectron Spectroscopy of ScN thin films (PC3 Src1). High resolution scans during the Ar ion etch (depth-profiles)." widths="450px" heights="400px" perrow="3">
image:eves_XPS_ScN_PC3_Src1_RF_Sc2p_and_N1s_2031019.png|Sc thin film XRR. Power: 200W, Deposition time: 500s, Pressure 3 mTorr. PC Gun Z-shift Position: Extended (95.20 mm).
image:eves_XPS_ScN_PC3_Src1_RF_Sc2p_and_N1s_2031019.png|<b>Sc 2p</b> and<b>N 1s</b> signals. 30 levels in total. 20s of etch with Ar<sup>+</sup> ions at low current and 1000eV energy between the measurements.
image:eves_XPS_ScN_PC3_Src1_RF_Sc_3s_2031019.png|Sc thin film XRR. Power: 200W, Deposition time: 750s, Pressure 3 mTorr. PC Gun Z-shift Position: Extended (95.20 mm).
image:eves_XPS_ScN_PC3_Src1_RF_Sc_3s_2031019.png|<b>Sc 3s</b> signal. 30 levels in total. 20s of etch with Ar<sup>+</sup> ions at low current and 1000eV energy between the measurements.
image:eves_XPS_ScN_PC3_Src1_RF_O_s1_2031019.png|Sc thin film XRR. Power: 200W, Deposition time: 750s, Pressure 3 mTorr. PC Gun Z-shift Position: Extended (95.20 mm).
image:eves_XPS_ScN_PC3_Src1_RF_O_s1_2031019.png|<b>O 1s</b> signal. 30 levels in total. 20s of etch with Ar<sup>+</sup> ions at low current and 1000eV energy between the measurements.
image:eves_XPS_ScN_PC3_Src1_RF_C_s1_2031019.png|Sc thin film XRR. Power: 200W, Deposition time: 1000s, Pressure 3 mTorr. PC Gun Z-shift Position: Extended (95.20 mm).
image:eves_XPS_ScN_PC3_Src1_RF_C_s1_2031019.png|<b>C 1s</b> signal. 30 levels in total. 20s of etch with Ar<sup>+</sup> ions at low current and 1000eV energy between the measurements.
</gallery>
</gallery>


<gallery caption="X-ray reflectivity scans of Sc thin films (PC3 Src1). " widths="450px" heights="400px" perrow="3">
<gallery caption="X-ray Photoelectron Spectroscopy of ScN thin films (PC3 Src1).  2-Dimensional depth profiles." widths="450px" heights="400px" perrow="3">
image:eves_XPS_2D_ScN_Sc2p_and_N1s_PC3_Src1_RF_20231018.png|Sc thin film XRR. Power: 200W, Deposition time: 500s, Pressure 3 mTorr. PC Gun Z-shift Position: Home (00.00 mm).
image:eves_XPS_2D_ScN_Sc2p_and_N1s_PC3_Src1_RF_20231018.png|2D profile of <b>Sc 2p</b> and <b>N 1s</b> signals. 30 levels in total. 20s of etch with Ar<sup>+</sup> ions at low current and 1000eV energy between the measurements.
image:eves_XPS_2D_ScN_Sc3s_PC3_Src1_RF_20231018.png|Sc thin film XRR. Power: 200W, Deposition time: 500s, Pressure 3 mTorr. PC Gun Z-shift Position: Home (00.00 mm).
image:eves_XPS_2D_ScN_Sc3s_PC3_Src1_RF_20231018.png|2D profile of <b>Sc 3s</b> signal. 30 levels in total. 20s of etch with Ar<sup>+</sup> ions at low current and 1000eV energy between the measurements.
image:eves_XPS_2D_ScN_O1s_PC3_Src1_RF_20231018.png|Sc thin film XRR. Power: 150W, Deposition time: 750s, Pressure 3 mTorr. PC Gun Z-shift Position: Home (00.00 mm).
image:eves_XPS_2D_ScN_O1s_PC3_Src1_RF_20231018.png|2D profile of <b>O 1s</b> signal. 30 levels in total. 20s of etch with Ar<sup>+</sup> ions at low current and 1000eV energy between the measurements.
image:eves_XPS_2D_ScN_C1s_PC3_Src1_RF_20231018.png|Sc thin film XRR. Power: 100W, Deposition time: 1000s, Pressure 3 mTorr. PC Gun Z-shift Position: Home (00.00 mm).
image:eves_XPS_2D_ScN_C1s_PC3_Src1_RF_20231018.png|2D profile of <b>C 1s</b> signal. 30 levels in total. 20s of etch with Ar<sup>+</sup> ions at low current and 1000eV energy between the measurements.
</gallery>
</gallery>


==Scanning Electron microscopy==
==Scanning Electron Microscopy==


The images below present SEM images of the ScN layers from the top and tilted view.  
The images below present [[Specific Process Knowledge/Characterization/SEM: Scanning Electron Microscopy |Scanning Electron Microscopy (SEM)]] images of the ScN layers from the top and tilted view.  


<gallery caption="Scanning Electron Microscopy." widths="480px" heights="400px" perrow="3">
<gallery caption="Scanning Electron Microscopy." widths="480px" heights="400px" perrow="3">
image:eves_SEM_ScN_3mTorr_1000s_200W_PC3_Src1_RF_ext_image1_20231013.png| <b><span style="color: red">ScN</span></b> layer deposited at 200 W RF power, 3mTorr, and 1000s. Gun Z-shift position is "Extended". Top view.
image:eves_SEM_ScN_3mTorr_1000s_200W_PC3_Src1_RF_ext_image1_20231013.png| <b><span style="color: red">ScN</span></b> layer deposited at 200 W RF power, 3mTorr, and 1000s. Gun Z-shift position is "Extended". Top view.
image:eves_SEM_ScN_3mTorr_1000s_200W_PC3_Src1_RF_ext_image2_20231013.png| <b><span style="color: red">ScN</span></b> layer deposited at 200 W RF power, 3mTorr, and 1000s. Gun Z-shift position is "Extended". Tilted view.  
image:eves_SEM_ScN_3mTorr_1000s_200W_PC3_Src1_RF_ext_image2_20231013.png| <b><span style="color: red">ScN</span></b> layer deposited at 200 W RF power, 3mTorr, and 1000s. Gun Z-shift position is "Extended". Tilted view.  
image:eves_SEM_ScN_3mTorr_1000s_200W_PC3_Src1_RF_ext_image3_20231013.png| <b><span style="color: red">ScN</span></b> layer deposited at 200 W RF power, 3mTorr, and 1000s. Gun Z-shift position is "Extended". Tilted view
image:eves_SEM_ScN_3mTorr_1000s_200W_PC3_Src1_RF_ext_image3_20231013.png| <b><span style="color: red">ScN</span></b> layer deposited at 200 W RF power, 3mTorr, and 1000s. Gun Z-shift position is "Extended". Tilted view
</gallery>
</gallery>

Latest revision as of 16:32, 9 November 2023

Feedback to this page: click here


This page is written by Evgeniy Shkondin @DTU Nanolab if nothing else is stated.
All images and photos on this page belongs to DTU Nanolab.
The fabrication and characterization described below were conducted in 2022 by Evgeniy Shkondin, DTU Nanolab.


This page presents the results of Scandium Nitride deposition using RF Reactive Sputtering in Sputter-System Metal-Nitride (PC3) commonly known as "Cluster Lesker". The deposition target is 4" Sc (0.250" Indium bonded with indium to 3mm Cu plate). Source #1 was used. Materials (ScN) from this source can either be deposited with RF or p-DC sputtering although only RF mode has been tested so far.


The main focus of the study was the deposition rate, optical functions, and the general performance of deposition from a bigger 4” target. The scandium nitride sputtering from the target of this size allows achieving a higher deposition rate and service to many potential applications where several hundreds of nm are needed to be put uniformly on a wafer of 150 mm or similar. Additionally, the flexibility of this source (z-shift and tilting) allows tailoring the deposition output.

The most common application of scandium is its use as a dopant or addition to aluminum in the deposition of AlScN thin films. The presence of scandium enhances the preffered crystallographic orientation of aluminum nitride (AlN) and significantly improves the overall piezoelectric performance of the thin film. With the Cluster Lesker tool (PC3), scandium can be loaded into Source 1, while aluminum can be loaded into Source 2. Co-sputtering can then be performed from both sources, allowing for precise adjustment of individual powers, gas flows, and other parameters. This flexibility enables the tailoring of thin film stoichiometry and other properties to meet specific requirements.

4” magnetron in PC3 has more functionalities compared to the ordinary guns in cluster Lesker. It can(to some degree) moves in Z-direction. This will affect the deposition rate, uniformity and most likely play an important role in reactive sputtering. Besides that, it can be easily tilted if necessary. In this study, two z-high positions have been compared (lowest-“home” and highest –“extended”). The effect of power has also been evaluated.

Note! It seems that Scandium is prone to oxidation, better to keep the prepared samples in a inert environment.


RF Sputtering of Scandium Nitride in Sputter-System Metal-Nitride(PC3)

The RF ScN process recipe in a Sputter-System Metal-Nitride(PC3) is following:

* Recipe Name:  MD PC3_Src1 - RF_Downstream with Reactive N2
  • PC Gun Z-shift Position: Home (00.00 mm) and Extended (95.20 mm)
  • Tilt: No (Target in horizontal plane)
  • Deposition mode: Downstream
  • Rotation speed: 10 rpm
  • Pressure: 3 mTorr
  • Power: 100-200 W (It is recommended to use 200W for getting high deposition rate and using "Extended" gun Z-shift position).
  • Ar flow: 40 sccm
  • N2 flow: 18 sccm
  • Deposition time: 1000 s
  • Deposition temperature: 400 °C
  • Pre-sputtering time : 300s (better to give longer time to sputter away the native oxide, especially on a recently installed target)


Samples: 6" Si without native oxide (HF-treated).

Deposition Rate

Scandium nitride deposition conditions
PC Gun Z-shift Position: Extended (95.20 mm).
Power (W) Pressure (mTorr) Time (s) Total Thickness (nm) Deposition rate (nm/s)
200 3 500 37.7

0.0754

150 3 750 25.0

0.0334

100 3 1000 14.1

0.0141

PC Gun Z-shift Position: Home (00.00 mm).
Power (W) Pressure (mTorr) Time (s) Total Thickness (nm) Deposition rate (nm/s)
200 3 500 16.6

0.0333

150 3 750 10.0

0.0133

100 3 1000 5.8

0.0058


X-ray Reflectivity (XRR)

X-ray Reflectivity analysis of ScN samples have been performed to investigate the thicknesses, roughness, and density profiles.

The scans has been obtained using Rigaku XRD SmartLab equipment. The voltage and current settings for the Cu X-ray tube were standard 40kV and 30mA. The incident optics contained a IPS (incident parallel slit) adaptor with 5 ° Soller slit. Other slits: IS=0.05mm RS1=0.05mm and RS2=0.075mm. Step size: 0.01 and measurement time - 5s for each point. Fitting procesure was performed using commercial GlobalFit software assuming the model based on Si substrate followed by Sc-Si transition layer for better fit, followed by the main ScN film with thin oxides and moisture surfaces. The results are summarized in a tables below.


Extracted values

XRR results for ScN thin films deposited at 3 mTorr and different powers. PC Gun Z-shift Position: Extended (95.20 mm)
Top layer (moisture) ScNxOy Main ScN layer Sc-Si intermediate layer Si substrate
Deposition name Moisture thickness (nm) Moisture density (g/cm3) Moisture roughness (nm) ScNxOy thickness (nm) ScNxOy density (g/cm3) ScNxOy roughness (nm) ScN thickness (nm) ScN density (g/cm3) ScN roughness (nm) Sc-Si intermediate layer thickness (nm) Sc-Si intermediate layer density (g/cm3) Sc-Si intermediate layer roughness (nm) Si thickness (nm) Si density (g/cm3) Si roughness (nm)
200W, 3mTorr, 1000s 1.33 0.60 0.15 0.43 2.73 0.72

37.28

4.82

1.87

0.75 2.87 0.92 2.33 0.03
150W, 3mTorr, 1000s 0.63 0.67 0.05 0.85 1.61 1.24

24.17

4.92

0.78

1.20 3.20 0.76 2.33 0.04
100W, 3mTorr, 1000s 1.69 0.19 0.00 1.63 2.99 0.51

12.43

4.83

0.00

2.06 1.97 1.27 2.33 0.00


XRR results for ScN thin films deposited at 3 mTorr and different powers. PC Gun Z-shift Position: Home (00.00 mm)
Top layer (moisture) ScNxOy Main ScN layer Sc-Si intermediate layer Si substrate
Deposition name Moisture thickness (nm) Moisture density (g/cm3) Moisture roughness (nm) ScNxOy thickness (nm) ScNxOy density (g/cm3) ScNxOy roughness (nm) ScN thickness (nm) ScN density (g/cm3) ScN roughness (nm) Sc-Si intermediate layer thickness (nm) Sc-Si intermediate layer density (g/cm3) Sc-Si intermediate layer roughness (nm) Si thickness (nm) Si density (g/cm3) Si roughness (nm)
200W, 3mTorr, 1000s 3.03 0.08 0.00 0.60 4.66 1.28

16.04

4.87

0.00

2.22 2.12 1.08 2.33 0.00
150W, 3mTorr, 1000s 1.29 1.17 0.00 0.53 2.71 1.28

9.44

4.42

0.08

1.25 2.94 0.48 2.33 0.03
100W, 3mTorr, 1000s 0.64 1.62 0.00 1.06 2.23 1.91

4.79

4.63

0.61

1.16 3.04 0.62 2.33 0.05



Fitting parameters
Sample Moisture ScNxOy ScN Sc-Si intermediate layer Si substrate Fitting parameters
Delta Beta Delta Beta Delta Beta Delta Beta Delta Beta Intensity Background Fitting area (2Θ) R X2
PC Gun Z-shift Position: Extended (95.20 mm) 200W, 3mTorr, 500s 1.9484E-6 4.5244E-8 8.9012E-6 2.0670E-7 1.3473E-5 1.2304E-6 9.3367E-6 2.1681E-7 7.5860E-6 1.7616E-7 1.30347E-000 3.58520E-007 0.4055 - 4.0000 0.01563 0.00513
PC Gun Z-shift Position: Extended (95.20 mm) 150W, 3mTorr, 750s 2.1902E-6 5.0859E-8 5.1589E-6 1.1980E-7 1.3736E-5 1.2545E-6 1.0416E-5 2.4187E-7 7.5860E-6 1.7616E-7 1.08491E-000 9.64995E-007 0.4055 - 4.0000 0.01452 0.00413
PC Gun Z-shift Position: Extended (95.20 mm) 100W, 3mTorr, 1000s 6.3024E-7 1.4635E-8 9.7505E-6 2.2642E-7 1.3484E-5 1.2314E-6 6.4131E-6 1.4892E-7 7.5860E-6 1.7616E-7 1.17155E-000 2.25376E-006 0.4055 - 4.0000 0.00744 0.00101
PC Gun Z-shift Position: Home (00.00 mm) 200W, 3mTorr, 500s 2.5771E-7 5.9844E-9 1.5175E-5 3.5239E-7 1.3596E-5 1.2417E-6 6.8990E-6 1.6020E-7 7.5860E-6 1.7616E-7 1.00181E-000 3.89203E-011 0.4055 - 4.0000 0.01830 0.00741
PC Gun Z-shift Position: Home (00.00 mm) 150W, 3mTorr, 750s 3.8018E-6 8.8284E-8 8.8171E-6 2.0475E-7 1.2333E-5 1.1264E-6 9.5589E-6 2.2197E-7 7.5860E-6 1.7616E-7 1.37654E-000 5.17162E-009 0.4055 - 4.0000 0.00825 0.00129
PC Gun Z-shift Position: Home (00.00 mm) 100W, 3mTorr, 1000s 5.2890E-6 1.2282E-7 7.1123E-6 1.6516E-7 1.2924E-5 1.1803E-6 1.0009E-5 2.3243E-7 7.5860E-6 1.7616E-7 1.19799E-000 1.15388E-006 0.4055 - 4.0000 0.00466 0.00039






X-ray Photoelectron Spectroscopy

X-ray Photo Electron Spectroscopy (XPS) was employed to investigate the chemical composition of deposited scandium nitride (ScN) thin films using the XPS K-Alpha instrument. The analysis was conducted in a 'depth profile' mode, where the film was incrementally etched, and the composition was measured layer by layer. Multiple scans were performed, including survey scans and scans for specific elements like O1s, N1s, Sc2p, Sc3s, and C1s, to gather comprehensive chemical information.

Interpreting the stoichiometry of the ScN film is challenging due to the overlap between the N1s peak and the Sc2p peak. Additionally, while scandium has various interesting electronic states that can be measured and utilized in calculations (such as Sc3s), there is only one electronic state for nitrogen, N1s, which requires careful deconvolution from the Sc2p peak.

The ScN sample used for XPS analysis was deposited at the PC Gun Z-shift Extended position (95.20mm) under the following conditions: 400°C, Ar/N 40/18 sccm, 200W power, 3mTorr pressure, and a deposition time of 1000 seconds.

Estimated stoichiometry is following: N=37.73%, Sc=48.11%, O=13.89%.

The Sc target used in the experiment was new, and due to its susceptibility to oxidation, there is a possibility of a pronounced level of Scandium oxynitride formation. We believe that more extensive usage of the target will remove the oxidized top layer. Additionally, it is necessary to perform preconditioning (pre-sputtering) of the target before using it in applications. This pre-sputtering process will help minimize the oxygen level in the resulting film.

Scanning Electron Microscopy

The images below present Scanning Electron Microscopy (SEM) images of the ScN layers from the top and tilted view.