| Q01: Last Friday I ran the first nanoetches with the recipe below - with limited success however. I was short on
| |
| time so I couldn't investigate it further but for some reason the coil power would rise to some 1500 W in the
| |
| first few seconds of the etch and og out of tolerance. I tried switching to forward power, no success. I
| |
| copied a switched recipe and adjusted all the parameters that I know to change and switched to continuous
| |
| tolerance recipe. What about matching, wouldn't it be good idea to try and run the process manually
| |
| (ramping up RF powers and allowing the matching network to stabilize and setting the load/tune parameters
| |
| as starting points?) and I don't need to strike the plasma...?
| |
|
| |
|
| A01:It is odd that the power delivery went up to 1500W when the demand was 800W. It sounds like the
| |
| matching needs to be looked at more closely. Careful set up of the starting positions will be needed; these
| |
| will likely be different to what has worked before in any other recipe as the conditions for this process are
| |
| quite different.
| |
|
| |
| It will be worth doing a trial run on a PR-coated or oxide wafer where a strike pressure of 20mT is allowed
| |
| just to get the plasma struck, then record the load and tune values when the pressure gets to the desired
| |
| 4mT and is running stable. The load and tune start points should then be set to values ~5% away from the
| |
| "sweet spot"; when the RF first comes on the transient in the impedance forces the matching unit to search -
| |
| we want the unit to search towards the sweet spot positions and not away from them - if the start point is
| |
| set to the best value then it will likely never match properly as the caps will drive away from these positions
| |
| as soon as the power comes through.
| |
|
| |
| There are two methods of achieving good matching:
| |
|
| |
| 1. Start points set to 5% below and 5% above the sweet spot on the Load and Tune respectively OR 2. The
| |
| Load set to start in the sweet spot position and Tune set 5% below
| |
| 4mT is a difficult pressure to strike at so it may be necessary to use the strike pressure anyway; only 3s of
| |
| plasma in 10-20mT strike pressure range should have little-to-no effect on the process result.
| |
|
| |
|
| |
|
| |
| Q02a:I have tried many times now and I can't find a stable, repeatable process. I would like you to comment on
| |
| the following facts/observations: I try to find a stable process on a 4" si wafer coated with AZ PR with 80 % exposed to plasma. The actual wafers are 2" Si wafers with some 100 nm ZEP resist and only very small nm-sized areas in the center and lying on 4" dummy wafer with 2" reces.
| |
|
| |
| A02a: This is an unusual mix. The set up wafer sounds fine - standard 100mm wafer with AZ PR coating.
| |
| The 2" wafer on 4" dummy is unusual in Pegasus (most Pegasus tools are at 150-200mm), I have completed
| |
| many process runs on mounted-wafer pieces using coogrease or crystalbond which would likely mimic your
| |
| set up. What is unusual is the "dummy wafer with 2" recess" - I am not sure what this is. Either way, this
| |
| should have no effect on the coil matching.
| |
|
| |
| Q02b: I don't know why the coil power shoots up (sometimes above 2000 W) in the very first seconds of the etch.
| |
| Adding a 15 second strike @ 15 mtorr, playing around with coil matching parameters (as suggested by you
| |
| below), using load or forward coil power or introducing 15 seconds gas stabilizations do not seem to make
| |
| much difference.
| |
|
| |
| A02b:The two datalogs you sent do not show any issue with reflected coil power in the first few seconds of
| |
| processing. There is no large reflected power spike and coil matching unit performance looks stable. 15s
| |
| gas stabilisation should ALWAYS be run - the most important part of the stabilisation is the homing of the
| |
| matching unit to ensure that the unit "knows" where the capacitors are at and also there is a physical HF/LF
| |
| switch in the platen matching which only changes during the stabilisation...i.e. a HF process run with no
| |
| stabilisation after a LF process would have the platen matching switch still set to LF. Without stabilisation,
| |
| there are likely to be matching issues on the coil and possibly on the platen depending on previous process
| |
| run.
| |
|
| |
| It is expected to see a reflected power spike at the start of the process as the plasma is being struck;
| |
| provided that this spike comes down very quickly there is usually no issue. Also, it is important that the
| |
| matching start points are set ~5% away from the "sweet spot" to ensure that the matching is repeatable run-
| |
| to-run during the transient phase as the plasma strikes; if the matching is not set up well, then it is a matter
| |
| of luck.....some runs will strike well, others will not.
| |
|
| |
|
| |
|
| |
| Q02c: Would it be a good idea to run a conditioning run before the wafers and after TDESC cleans. I have tried
| |
| to make a conditioning recipe with a ramping step where the coil power is ramped from 300 to 800 W in 30
| |
| seconds in order for the matching unit to find the sweet spot more easily before a 'non-ramped' step.
| |
|
| |
| A02c: Provided usual inter-wafer (waferless) clean protocol is followed, there should be no need for specific
| |
| conditioning runs. It may be worth running a few minutes of the desired process when switching from a very
| |
| different process window but there should be little/no difference provided a 3minute interwafer clean is run
| |
| immediately before any process run. To clarify:
| |
| In "development mode" (only few-several runs per day) 3minute clean before the process run is
| |
| needed.
| |
| In "production mode" (continuous running of batch processes), 3minute clean at the very start followed
| |
| by interwafer clean
| |
| (time of interwafer clean should follow a rough rule of thumb of ~3s clean/minute of actual
| |
| processing + ~10% if process time is longer than a few minutes, otherwise, for very short processes a
| |
| batch clean of ~30minutes to 1hr depending on duration of batch process).
| |
|
| |
| Q02d: My colleague Berit who is working hard to find the right Cr etch on our ICP metal etcher has just been
| |
| informed that due to the usage of the '10% range' option on the platen power her processes have been
| |
| running with 10 times as much platen power as intended. In my experiments so far I have seen that the 100
| |
| nm of ZEP resist is gone after 30 seconds of processing...
| |
|
| |
| A02d: I'm not sure of the details on the metal etcher. On the Pegasus, selecting 10% range will limit the range
| |
| to 30W, selecting "full" will allow up to 300W. You are running 50W with this process - the range should
| |
| be set to full. If running <30W, then setting full range will not deliver 10x more power than requested, just
| |
| that the control of fwd power will not be as accurate as if 10% range is selected (i.e. 0-5V = 0-30W in 10%
| |
| range, 0-5V = 0-300W in full range). I think that on the metal etcher there is an issue due to the different
| |
| platen generator. It is worth double-checking the generator display on the Pegasus when running low
| |
| power and 10% range selected as this is a combination not very often used.
| |
|
| |
| 100nm of ZEP resist is not much and it is feasible to think that this is stripping off in 30s of process time. ZEP
| |
| resist will show a much lower selectivity than standard resist. The conditions are going to be quite hard on
| |
| the mask - low pressure and relatively high platen power. Use of ZEP resist and the process conditions you
| |
| are running is very rare in the Pegasus - it is difficult to say what you should expect to see.
| |
|
| |
| How is the 2" wafer bonded to the carrier and what is the carrier? If thermal bonding is not good such that
| |
| the cooling is lost or not efficient, then there will be lack of deposition on the mounted wafer resulting in
| |
| low selectivity.
| |
|
| |
| Q02e: I have attached the recipes that I am using - can you find any bad parameters?
| |
|
| |
| A02e: Aside from the lack of stabilisation in some of the recipes and use of 10% range in platen power (which
| |
| will probably limit forward power to 30W when demand is 50W), I cannot see anything wrong with the
| |
| processes.
| |