===GaAs/AlGaAs etching using III-V ICP===
===GaAs/AlGaAs etching using III-V ICP===
'''''Work done by DTU Photonics before 2011'''''
'''''Recipes developed and/or tested by DTU Photonics internal before 2011'''''


{| border="1" cellspacing="2" cellpadding="3"  
{| border="1" cellspacing="2" cellpadding="3"  
Line 24: Line 24:
|-
|-
|Platen chiller  temperature
|Platen chiller  temperature
|20 <sup>o</sup>C
|20<sup>o</sup>C
|-
|-
|}
|}
Line 36: Line 36:
|-
|-
|Sidewall angle
|Sidewall angle
|~ 85-90 <sup>o</sup>
|~ 85-90<sup>o</sup>
|-
|-
|Selectivity (GaAs:Si<sub>3</sub>N<sub>4</sub>, GaAs:AlInP)  
|Selectivity (GaAs:Si<sub>3</sub>N<sub>4</sub>, GaAs:AlInP)  
Line 64: Line 64:
|-
|-
|Platen chiller  temperature
|Platen chiller  temperature
|20 <sup>o</sup>C
|20<sup>o</sup>C
|-
|-
|}
|}
Line 76: Line 76:
|-
|-
|Sidewall angle
|Sidewall angle
|~ 90 <sup>o</sup>
|~ 90<sup>o</sup>
|-
|-
|Selectivity (GaAs:SiO<sub>2</sub>)  
|Selectivity (GaAs:SiO<sub>2</sub>)  
Line 110: Line 110:
|-
|-
|Platen chiller  temperature
|Platen chiller  temperature
|20 <sup>o</sup>C
|20<sup>o</sup>C
|-
|-
|}
|}
Line 122: Line 122:
|-  
|-  
|Sidewall angle
|Sidewall angle
|85-90 <sup>o</sup>
|85-90<sup>o</sup>
|-
|-
|Selectivity (GaAs:Si<sub>3</sub>N<sub>4</sub>, GaAs:AlInP)  
|Selectivity (GaAs:Si<sub>3</sub>N<sub>4</sub>, GaAs:AlInP)  
Line 135: Line 135:


{| border="1" cellspacing="2" cellpadding="3"  
{| border="1" cellspacing="2" cellpadding="3"  
![[image:ICP_BCL3_result.jpg|300x300px|thumb|left|Result of GaAs etching with BCl<sub>3</sub>. Qijiang Ran, DTU Photonics, 2011. ]]
![[image:ICP_BCL3_result.jpg|300x300px|thumb|left|Result of GaAs etching with BCl<sub>3</sub>. Done by: Qijiang Ran, DTU Photonics, 2011. ]]
|-
|-
|}
|}

Latest revision as of 11:47, 4 September 2025

Feedback to this page: click here

GaAs/AlGaAs etching using III-V ICP

Recipes developed and/or tested by DTU Photonics internal before 2011

Recipe GaAs Etch
Cl2 flow 4 sccm
Ar flow 12 sccm
Platen power 80 W
Coil power 700 W
Pressure 6 mTorr
Platen chiller temperature 20oC


Results (GaAs Etch)
GaAs etch rate >500 nm/min
Sidewall angle ~ 85-90o
Selectivity (GaAs:Si3N4, GaAs:AlInP) 10:1, 5:1


Recipe GaAs_AlGaAs Etch
Cl2 flow 20 sccm
N2 flow 50 sccm
Platen power 100 W
Coil power 600 W
Pressure 2 mTorr
Platen chiller temperature 20oC


Results (GaAs_AlGaAs Etch)
AlGaAs etch rate >1000 nm/min
Sidewall angle ~ 90o
Selectivity (GaAs:SiO2) 30:1


Recipe GaAs_AlGaAs Etch_BCl3
Cl2 flow 10 sccm
BCl3 flow 10 sccm
Ar flow 10 sccm
N2 flow 4 sccm
Platen power 50 W
Coil power 500 W
Pressure 1 mTorr
Platen chiller temperature 20oC


Results (GaAs_AlGaAs Etch_BCl3)
GaAs etch rate >750 nm/min
Sidewall angle 85-90o
Selectivity (GaAs:Si3N4, GaAs:AlInP) 10:1
Result of GaAs etching with BCl3. Done by: Qijiang Ran, DTU Photonics, 2011.