Jump to content

Specific Process Knowledge/Etch/Wet Platinum Etch: Difference between revisions

Kabi (talk | contribs)
Hvje (talk | contribs)
mNo edit summary
 
(3 intermediate revisions by 2 users not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:wetchemistry@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Etch/Wet_Platinum_Etch click here]'''
'''Feedback to this page''': '''[mailto:wetchemistry@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/Wet_Platinum_Etch click here]'''
 
'''Unless anything else is stated, everything on this page, text and pictures are made by DTU Nanolab.'''
 
'''All links to Kemibrug (SDS) and Labmanager Including APV requires login.'''
 
'''All measurements on this page has been made by Nanolab staff.'''  


Etching of Platinum can be done either wet or dry. For wet etching please see below on this page. Dry etching can be done with [[Specific Process Knowledge/Etch/IBE/IBSD Ionfab 300|IBE]] by sputtering with Ar ions.  
Etching of Platinum can be done either wet or dry. For wet etching please see below on this page. Dry etching can be done with [[Specific Process Knowledge/Etch/IBE/IBSD Ionfab 300|IBE]] by sputtering with Ar ions.  
Line 10: Line 16:


*H<sub>2</sub>O : HCl : HNO<sub>3</sub>        (8 : 7 : 1) at 85 °C (note: etching starts at 70 C, 170nm etched in 5 min 70 C-85 C)* Nisoer July 2022
*H<sub>2</sub>O : HCl : HNO<sub>3</sub>        (8 : 7 : 1) at 85 °C (note: etching starts at 70 C, 170nm etched in 5 min 70 C-85 C)* Nisoer July 2022
'''You have to be very careful when you work with this etch. It can generate nitrous oxides which are very toxic!!'''
'''You have to be very careful when you work with this etch. It can generate nitrous gasses which are very toxic!!'''


At this moment we do not have any information on the etch rate. You should be aware that this wet etch will also etch gold and it is not possible to use any masking material, it is used as a stripper.
At this moment we do not have any information on the etch rate. You should be aware that this wet etch will also etch gold and it is not possible to use any masking material, it is used as a stripper.


Wet etching of Platinum is done by making your own setup in a glass beaker in Fumehood 01 or 02 in Cleanroom D-3. Write content on the beaker and which metals has been etched with yellow permanent pen. You can see the APV  [http://labmanager.dtu.dk/d4Show.php?id=4748&mach=368 here].
Wet etching of Platinum is done by making your own setup in a glass beaker in Fumehood 01 or 02 in Cleanroom D-3. Write content on the beaker and which metals has been etched with yellow permanent pen. Be aware that no other processes can be done in the fumehood at the same time.You can see the APV  [http://labmanager.dtu.dk/d4Show.php?id=4748&mach=368 here].


===Platinum Etch data===
===Platinum Etch data===