Jump to content

Specific Process Knowledge/Thin film deposition/Deposition of Tungsten: Difference between revisions

From LabAdviser
Eves (talk | contribs)
Eves (talk | contribs)
No edit summary
 
(16 intermediate revisions by 2 users not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:pvd@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Tungsten&action=edit click here]'''  
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Tungsten click here]'''


= Tungsten deposition =
<i> This page is written by <b>DTU Nanolab staff</b></i>


Tungsten (W) can be deposited by e-beam evaporation and sputtering. However, in case of evaporation the precess generates a lot of heat (despite water cooling), and this means the pressure rises as the chamber is baking out. It is therefore not easy to deposit films much thicker than 50-60 nm. In the Temescal we stopped the deposition every 20 nm to let the pressure drop. Also, the rate needs to be low, to avoid overheating. Talk to staff when you want to deposit W (write to thinfilm@nanolab.dtu.dk). Sputtering can be used without any sufficient issues. In the chart below you can compare the deposition equipment.
=Tungsten (W)=


==Sputtering of W==
Tungsten (W) is a refractory metal with the highest melting point of any element, remarkable density, hardness, and outstanding resistance to radiation and corrosion, making it indispensable in semiconductor, optical, and harsh‑environment technologies.
Thin films are produced primarily by magnetron sputtering or e-beam evaporation, yielding dense, low-resistivity body-centered-cubic α-W when pressure, substrate temperature, and energy are adequately controlled.
Within semiconductor process flows, α‑W serves as a robust diffusion‑barrier/liner, gate or contact metal, and reliable via/plug fill for logic, memory, and power devices operating at elevated temperatures.
In optics, the metal’s high atomic number and thermal stability underpin multilayer W/Si or W/C stacks used in X‑ray mirrors—such as Göbel mirrors, Kirkpatrick–Baez optics, synchrotron beamline monochromators, and space‑borne telescope coatings—delivering high reflectivity and power‑handling in the soft-to-hard-X-ray range.
α‑W also supports high‑temperature plasmonic and thermally emissive coatings, mid‑IR absorbers, and durable metamaterial surfaces that endure far greater power densities than noble metals.
Beyond electronics and photonics, tungsten’s mechanical strength and radiation tolerance enable MEMS springs, X‑ray/EUV shielding, high‑temperature sensors, and dense protective components; moreover, α‑W becomes superconducting at millikelvin temperatures, allowing niche low‑loss microwave resonators and detector elements where extreme stability is required.
 
== Tungsten deposition ==
 
Tungsten (W) can be deposited by e-beam evaporation and sputtering. However, in the case of evaporation, the process generates a lot of heat, so it is not easy to deposit films much thicker than 50-60 nm. Sputtering can be used without any particular issues. In the chart below, you can compare the deposition equipment.
 
===Evaporation of W===
 
*[[/Evaporation of W in Temescal|E-beam evaporation of Tungsten in the Temescal]]
 
===Sputtering of W===


*[[/Sputtering of W in Sputter Coater 3|Sputtering of Tungsten in the Sputter Coater 3]]
*[[/Sputtering of W in Sputter Coater 3|Sputtering of Tungsten in the Sputter Coater 3]]
 
*[[/DC Sputtering of W in Sputter-System (Lesker)|DC Sputtering of Tungsten in the Sputter-System (Lesker)]]
*[[/DC Sputtering of W in Sputter-system Metal-Nitride (PC3)|DC Sputtering of Tungsten in the Sputter-system Metal-Nitride (PC3)]]
*[[/HiPIMS Sputtering of W in Sputter-system Metal-Nitride (PC3)|HiPIMS Sputtering of Tungsten in the Sputter-system Metal-Nitride (PC3)]]




Line 23: Line 40:
! General description
! General description
| E-beam evaporation of W
| E-beam evaporation of W
| Sputtering of W
| DC Sputtering of W
| Sputtering of W
| DC and HiPIMS Sputtering of W
| Sputtering of W
| DC Sputtering of W
|-
|-
|-style="background:Lightgrey; color:black"
|-style="background:Lightgrey; color:black"
Line 31: Line 48:
|Ar ion beam
|Ar ion beam
|None
|None
|Ar ion beam
|RF bias on a substrate
|None
|None
|-
|-
Line 40: Line 57:
|10Å to 600nm  
|10Å to 600nm  
|10Å to 600nm  
|10Å to 600nm  
|10Å to 600nm
|10Å to 250nm
|-
|-


Line 48: Line 65:
|about 1 Å/s
|about 1 Å/s
|about 1 Å/s
|about 1 Å/s
|about 1 Å/s
|configuration dependent
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
! Batch size
! Batch size
Line 60: Line 77:
*small pieces
*small pieces
|
|
*Up to 1x4" wafers
*Up to 10x4" wafers
*Up to 1x6" wafer
*Up to 10x6" wafer
*small pieces
*small pieces
|
|
*Up to 1x4" wafers
*Up to 1x4" wafers
*Up to 1x6" wafer
*small pieces
*small pieces
|-
|-
Line 115: Line 131:
| Substrate gets hot during deposition  
| Substrate gets hot during deposition  
(for a 60 nm film it rose above 123 C)
(for a 60 nm film it rose above 123 C)
Wait for low base pressure (3-5 10<sup>-7</sup> Torr)
 
|Deposition rate is 0.083 nm/s for 150W and 3mTorr
Wait for low base pressure before start (3-5 10<sup>-7</sup> Torr)
|Deposition rate is 0.083 nm/s for 150W and 3mTorr
|Deposition rate is 0.107 nm/s for 150W and 3mTorr (Src3, DC)
|Deposition rate is 0.083 nm/s for 150W and 3mTorr
|Deposition rate is 0.124 nm/s for 140W and 3mTorr (PC3, Src3 DC),
 
(0.04 nm/s using HiPIMS - PC3, Src3)
|Note! Bad uniformity.
 
Deposition rate is 0.03 nm/s using big glass chamber.
 
Deposition rate is 0.2-0.9 nm/s (current dependent) using small glass chamber.
|}
|}


'''*''' ''For thicknesses above 20 nm talk to staff (write to thinfilm@nanolab.dtu.dk), as the heat and subsequent pressure rise means the deposition needs to be carried out in steps.''
'''*''' ''For thicknesses above 20 nm talk to staff (write to thinfilm@nanolab.dtu.dk), as the heat and subsequent pressure rise means the deposition needs to be carried out in steps.''

Latest revision as of 11:49, 29 July 2025

Feedback to this page: click here

This page is written by DTU Nanolab staff

Tungsten (W)

Tungsten (W) is a refractory metal with the highest melting point of any element, remarkable density, hardness, and outstanding resistance to radiation and corrosion, making it indispensable in semiconductor, optical, and harsh‑environment technologies. Thin films are produced primarily by magnetron sputtering or e-beam evaporation, yielding dense, low-resistivity body-centered-cubic α-W when pressure, substrate temperature, and energy are adequately controlled. Within semiconductor process flows, α‑W serves as a robust diffusion‑barrier/liner, gate or contact metal, and reliable via/plug fill for logic, memory, and power devices operating at elevated temperatures. In optics, the metal’s high atomic number and thermal stability underpin multilayer W/Si or W/C stacks used in X‑ray mirrors—such as Göbel mirrors, Kirkpatrick–Baez optics, synchrotron beamline monochromators, and space‑borne telescope coatings—delivering high reflectivity and power‑handling in the soft-to-hard-X-ray range. α‑W also supports high‑temperature plasmonic and thermally emissive coatings, mid‑IR absorbers, and durable metamaterial surfaces that endure far greater power densities than noble metals. Beyond electronics and photonics, tungsten’s mechanical strength and radiation tolerance enable MEMS springs, X‑ray/EUV shielding, high‑temperature sensors, and dense protective components; moreover, α‑W becomes superconducting at millikelvin temperatures, allowing niche low‑loss microwave resonators and detector elements where extreme stability is required.

Tungsten deposition

Tungsten (W) can be deposited by e-beam evaporation and sputtering. However, in the case of evaporation, the process generates a lot of heat, so it is not easy to deposit films much thicker than 50-60 nm. Sputtering can be used without any particular issues. In the chart below, you can compare the deposition equipment.

Evaporation of W

Sputtering of W


E-beam evaporation (Temescal) Sputter-system (Lesker) Sputter deposition ((Sputter-system Metal-Oxide (PC1) and Sputter-system Metal-Nitride (PC3)) ) Sputter coater (Sputter coater 03)
General description E-beam evaporation of W DC Sputtering of W DC and HiPIMS Sputtering of W DC Sputtering of W
Pre-clean Ar ion beam None RF bias on a substrate None
Layer thickness 10Å to 20nm* 10Å to 600nm 10Å to 600nm 10Å to 250nm
Deposition rate 0.5 Å/s to 1 Å/s about 1 Å/s about 1 Å/s configuration dependent
Batch size
  • Up to 4x6" wafers
  • Up to 3x8" wafers (ask for holder)
  • small pieces
  • Up to 1x4" wafers
  • Up to 1x6" wafer
  • small pieces
  • Up to 10x4" wafers
  • Up to 10x6" wafer
  • small pieces
  • Up to 1x4" wafers
  • small pieces
Allowed materials
  • Silicon
  • Silicon oxide
  • Silicon (oxy)nitride
  • Photoresist
  • PMMA
  • Mylar
  • SU-8
  • Metals
  • Silicon
  • Silicon oxide
  • Silicon (oxy)nitride
  • Photoresist
  • PMMA
  • Mylar
  • SU-8
  • Metals
  • Silicon
  • Silicon oxide
  • Silicon (oxy)nitride
  • Photoresist
  • PMMA
  • Mylar
  • SU-8
  • Metals
  • Silicon
  • Silicon oxide
  • Silicon (oxy)nitride
  • Photoresist
  • PMMA
  • Mylar
  • SU-8
  • Metals
Comments Substrate gets hot during deposition

(for a 60 nm film it rose above 123 C)

Wait for low base pressure before start (3-5 10-7 Torr)

Deposition rate is 0.107 nm/s for 150W and 3mTorr (Src3, DC) Deposition rate is 0.124 nm/s for 140W and 3mTorr (PC3, Src3 DC),

(0.04 nm/s using HiPIMS - PC3, Src3)

Note! Bad uniformity.

Deposition rate is 0.03 nm/s using big glass chamber.

Deposition rate is 0.2-0.9 nm/s (current dependent) using small glass chamber.

* For thicknesses above 20 nm talk to staff (write to thinfilm@nanolab.dtu.dk), as the heat and subsequent pressure rise means the deposition needs to be carried out in steps.