Jump to content

Specific Process Knowledge/Etch/DRIE-Pegasus/DREM/DREM 3kW 100% b: Difference between revisions

From LabAdviser
Jmli (talk | contribs)
No edit summary
Jmli (talk | contribs)
No edit summary
 
(One intermediate revision by the same user not shown)
Line 1: Line 1:
<!-- Page reviewed 9/8-2022 jmli -->
<!-- Page reviewed 9/8-2022 jmli -->
 
<!--Checked for updates on 4/4-2025 - ok/jmli -->


{| border="2" cellpadding="0" cellspacing="0" style="text-align:center;"
{| border="2" cellpadding="0" cellspacing="0" style="text-align:center;"
Line 16: Line 16:
! width="40" | Comments
! width="40" | Comments
! width="400" |SEM images
! width="400" |SEM images
! width="400" |Picoscope  
! width="40" |Picoscope  
! width="400" |Numbers  
! width="400" |Numbers  
|-
|-

Latest revision as of 08:41, 4 April 2025


Date Substrate Information Process Information Results
Wafer info Material/ Exposed area Condi- tioning Recipe Wafer ID Comments SEM images Picoscope Numbers
29/11-2019 Medusa One Si / 10% stab-19 chamber clean 20 nanolab/ jmli /DREM 3.0 kW 100% b S018653 Process log entry

SEM image: a000 a001 a002 a003 a004 a005 a006 a007 a008 a009 a010 a011 a012 a013
Trench width (um) 159.77 401.82 251.88 250.36 158.96 99.72 61.82 40.77 32.13 25.67 12.84 7.24 4.13 2.6
Etched depth (um) 145.56 145.42 145.8 147.62 146.52 142.74 136.64 128.65 123.88 118.18 100.34 84.65 69.04 60.36
Etch rate (um/min) 14.56 14.54 14.58 14.76 14.65 14.27 13.66 12.86 12.39 11.82 10.03 8.46 6.9 6.04
Etch rate (nm/cyc) 1.21 1.21 1.21 1.23 1.22 1.19 1.14 1.07 1.03 0.98 0.84 0.71 0.58 0.5
Sidewall bowing (%) -0.28 -0.51 -0.38 -0.38 -0.4 0.05 0.18 -0.14 0.09 0.19 0.36 0.45 0.52 0.53
Sidewall angle (degs) 92.65 93.1 92.66 93.02 92.84 92.17 92.04 91.86 91.92 91.7 91.52 91.05 90.71 90.61
Bottom bowing (%) 8.1 3.9 6.18 6.71 9.14 10.53 14.26 17.43 16 16.76 15.69 16.18 14.53 11.69
Aspect ratio 0.87 0.35 0.56 0.57 0.88 1.36 2.05 2.86 3.41 4.05 6.47 9.64 13.86 18.56