== Results at 30 kV (Raith eLINE) ==
A dose test is carried out with the following parameters
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;"  style="width: 95%"
|-
|-
|-style="background:Black; color:White"
!colspan="5"|AR-N 8200 30 kV dose test, Processed by THOPE, AUG 2022
|-
|-
|-style="background:WhiteSmoke; color:black"
!Resist
!Spin Coat
!E-beam exposure
!PEB
!Development
|-
|-
|-style="background:WhiteSmoke; color:black"
|AR-N8200.06
|LabSpin 2, 4000 rpm for 60s, softbake 10 min @ 150 degC, thickness is 120 nm
|Raith eLINE Plus, 30 kV, 60 µm aperture, 168 pA
|Labspin 2 hotplate 170 degC for 10 min
|EBL development fumehood, 60 sec development in AR300-47:DIW (1:1), 30 sec rinse in DIW, nitrogen gun dry
|-
|}
Area/curved element dose: Fully insoluble dose is around 150-180 µC/cm2.
Line dose: Fully insoluble dose is around 1700 pC/cm.
Dot dose: Fully insoluble dose is around 0.1 pC, this gives a circular diameter of 60 nm. Diameter can be varied by increasing dose, at 0.4 pC diameter is about 100 nm and at 1.2 pC it is about 170 nm.