Jump to content

Specific Process Knowledge/Thin film deposition/Deposition of Germanium: Difference between revisions

From LabAdviser
Reet (talk | contribs)
Reet (talk | contribs)
 
(10 intermediate revisions by 2 users not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Germanium click here]'''
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Germanium click here]'''


''All text by DTU Nanolab staff''


== Deposition of Germanium ==
== Deposition of Germanium ==
Germanium can be deposited by thermal evaporation, e-beam evaporation, and sputtering.
Germanium can be deposited by thermal evaporation, e-beam evaporation, and sputtering.


==Thermal deposition==
==Resistive Thermal evaporation==
* [[/Thermal Ge deposition Wordentec|Thermal deposition of Ge in Wordentec]]


Current process information on Ge thermal evaporation:
* [[/Thermal Ge evaporation Thermal Evaporator|Resistive thermal evaporation of Ge in Thermal Evaporator - Lesker]]
Some very instrument specific deposition parameters for a now-decommissioned tool can be found here: [[/Thermal Ge deposition Wordentec|Thermal deposition of Ge in Wordentec]]


==Ge deposition equipment comparison==
==Ge deposition equipment comparison==
Line 16: Line 20:
|-style="background:silver; color:black"
|-style="background:silver; color:black"
!  
!  
! Thermal evaporation ([[Specific Process Knowledge/Thin film deposition/Wordentec|Wordentec]])
! Thermal evaporation ([[Specific Process Knowledge/Thin film deposition/thermalevaporator|Thermal Evaporator]])
! E-beam evaporation ([[Specific Process Knowledge/Thin film deposition/Physimeca|Physimeca]])
! E-beam evaporation ([[Specific Process Knowledge/Thin film deposition/Temescal|E-beam evaporator (Temescal)]] and [[Specific Process Knowledge/Thin film deposition/10-pocket e-beam evaporator|E-beam evaporator (10-pockets)]])
! E-beam evaporation ([[Specific Process Knowledge/Thin film deposition/Temescal|Temescal]])
! Sputtering ([[Specific Process Knowledge/Thin film deposition/Lesker|Lesker]])
! Sputtering ([[Specific Process Knowledge/Thin film deposition/Lesker|Lesker]])
! Sputtering ([[Specific Process Knowledge/Thin film deposition/Cluster-based multi-chamber high vacuum sputtering deposition system|Sputter-system Metal-Oxide (PC1) and Sputter-system Metal-Nitride (PC3)]])
! Sputtering ([[Specific Process Knowledge/Thin film deposition/Cluster-based multi-chamber high vacuum sputtering deposition system|Sputter-system Metal-Oxide (PC1) and Sputter-system Metal-Nitride (PC3)]])
Line 26: Line 29:
! General description
! General description
|Thermal deposition of Ge
|Thermal deposition of Ge
|E-beam deposition of Ge
|E-beam deposition of Ge
|E-beam deposition of Ge
|Sputter deposition of Ge
|Sputter deposition of Ge
Line 36: Line 38:
|-style="background:LightGrey; color:black"
|-style="background:LightGrey; color:black"
! Pre-clean
! Pre-clean
|RF Ar clean
 
| -
|none
|Ar ion beam clean
|Ar ion etch (only in E-beam evaporator Temescal)
|RF Ar clean
|RF Ar clean
|RF Ar clean
|RF Ar clean
|-
|-
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
! Layer thickness
! Layer thickness
|10Å to about 2000Å (in total distributed on all loaded wafers)
|10 Å to about 2000 Å
|10Å to about 3000Å
|few nm to about 1 µm*
|10Å to about 1000 nm
|10 Å to at least 1000 Å
|10Å to at least 1000 Å
|10 Å to ?
|10Å to ?
|-
|-
|-style="background:LightGrey; color:black"
|-style="background:LightGrey; color:black"
! Deposition rate
! Deposition rate
|From 0.4 Å/s up to about ~2Å/s
|1 Å/s  
|5 Å/s
|1 Å/s - 5 Å/s  
|From 1 Å/s up to 5 Å/s  
|Depends on deposition parameters
|Depends on deposition parameters
|Depends on deposition parameters
|Depends on deposition parameters
Line 62: Line 63:
! Batch size
! Batch size
|
|
*24x 2" wafers or  
*4x 2" wafers or  
*6x 4" wafers or
*3x 4" wafers or
*6x 6" wafers or
*1x 6" wafers or
*1x 8" wafers or
Many small pieces
Many small pieces
|
*1x 2" wafer or
*1x 4" wafers or
*Several smaller pieces
|
|
*Up to 4 x 6" wafer or
*Up to 4 x 6" wafer or
Line 88: Line 86:
|-style="background:LightGrey; color:black"
|-style="background:LightGrey; color:black"


! Allowed substrates
! Allowed materials
|
|
* Silicon wafers
Almost any that does not degas. See the [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=404 cross-contamination sheet].
* Quartz wafers
* Pyrex wafers
|
|
* III-V materials
Almost any that does not degas at your intended substrate temperature. See the [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=511 cross-contamination sheet].
* Silicon wafers
* Quartz wafers
* Pyrex wafers
|
|
*Silicon wafers
*Almost any that does not degas at your intended substrate temperature.  
*Quartz wafers
*Pyrex wafers
*See also the [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=429 cross-contamination sheet]
 
|
|
*Almost any that does not degas at your intended substrate temperature. See also the cross-contamination sheet
*Almost any that does not degas at your intended substrate temperature. See cross contamination sheets for [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=441 PC1] and [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=442 PC3]
|
*Almost any that does not degas at your intended substrate temperature. See also the cross-contamination sheets
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"


!Allowed materials


|
* Silicon oxide
* Silicon (oxy)nitride
* Photoresist
* PMMA
* Mylar
* SU-8
* Metals
|
* Silicon oxide
* Silicon (oxy)nitride
* Photoresist
* PMMA
* Mylar
|
*Silicon oxide
*Silicon (oxy)nitride
*Photoresist
*PMMA
*Mylar
*Metals
*See also the [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=429 cross-contamination sheet]
|
*Almost any as above
|
*Almost any as above
|-style="background:LightGrey; color:black"
! Comment
|Recommended for unexposed e-beam resist
|
|
|
|
|}
|}
'''*'''  ''For cumulative deposition above 600 nm please write to metal@nanolab.dtu.dk to make sure there will be enough material present in the machine.

Latest revision as of 00:27, 8 July 2025

Feedback to this page: click here

All text by DTU Nanolab staff

Deposition of Germanium

Germanium can be deposited by thermal evaporation, e-beam evaporation, and sputtering.

Resistive Thermal evaporation

Current process information on Ge thermal evaporation:

Some very instrument specific deposition parameters for a now-decommissioned tool can be found here: Thermal deposition of Ge in Wordentec

Ge deposition equipment comparison


Thermal evaporation (Thermal Evaporator) E-beam evaporation (E-beam evaporator (Temescal) and E-beam evaporator (10-pockets)) Sputtering (Lesker) Sputtering (Sputter-system Metal-Oxide (PC1) and Sputter-system Metal-Nitride (PC3))
General description Thermal deposition of Ge E-beam deposition of Ge Sputter deposition of Ge Sputter deposition of Ge
Pre-clean none Ar ion etch (only in E-beam evaporator Temescal) RF Ar clean RF Ar clean
Layer thickness 10 Å to about 2000 Å few nm to about 1 µm* 10 Å to at least 1000 Å 10 Å to ?
Deposition rate 1 Å/s 1 Å/s - 5 Å/s Depends on deposition parameters Depends on deposition parameters
Batch size
  • 4x 2" wafers or
  • 3x 4" wafers or
  • 1x 6" wafers or
  • 1x 8" wafers or

Many small pieces

  • Up to 4 x 6" wafer or
  • 3x 8" wafers (ask for special holder)
  • Many smaller pieces
  • 1x6" wafer or
  • 1x4" wafer or

smaller pieces

  • 10x6" or 4" wafers
  • many smaller pieces
Allowed materials

Almost any that does not degas. See the cross-contamination sheet.

Almost any that does not degas at your intended substrate temperature. See the cross-contamination sheet.

  • Almost any that does not degas at your intended substrate temperature.
  • Almost any that does not degas at your intended substrate temperature. See cross contamination sheets for PC1 and PC3

* For cumulative deposition above 600 nm please write to metal@nanolab.dtu.dk to make sure there will be enough material present in the machine.