Jump to content

Specific Process Knowledge/Thin film deposition/Deposition of Tin: Difference between revisions

BGE (talk | contribs)
No edit summary
Reet (talk | contribs)
 
(16 intermediate revisions by 6 users not shown)
Line 1: Line 1:
Tin can be deposited by e-beam evaporation. In the chart below you can compare the different deposition equipment.
= Tin Deposition =


Tin can be deposited by sputtering, thermal evaporation or e-beam evaporation in DTU Nanolab's cleanroom.


{| border="1" cellspacing="0" cellpadding="4"  
==Sputtering of tin==
We have sputtered tin in both the [[Specific Process Knowledge/Thin film deposition/Lesker|Sputter system (Lesker)]] and the [[Specific Process Knowledge/Thin film deposition/Cluster-based multi-chamber high vacuum sputtering deposition system|Sputter-system Metal-Oxide (PC1)]]. In the former we have also tested co-sputtering with Cu. In the latter we have more recent results (2025). The initial films were quite rough. Please contact staff for more information.
 
==E-beam evaporation of tin==
Sn was evaporated in the Alcatel e-beam evaporator, which is decommissioned, but has only been tested once in the [[Specific Process Knowledge/Thin film deposition/Temescal|E-beam evaporator (Temescal)]] which is currently in the lab. The test resulted in a rather uneven film (more resembling islands of Sn than a continuous layer) and since results with sputtering were more promising we did not fully develop the recipe (spring 2025).
 
==Thermal evaporation of tin ==
Sn thermal evaporation has been tested in early 2025. The required power varied quite a lot from run to run so we do not have a fully automated reliable process. The resulting films were very rough.
 
==Comparison of deposition methods==
{| border="1" cellspacing="0" cellpadding="3"
|-style="background:silver; color:black"
!  
!  
! E-beam evaporation ([[Specific Process Knowledge/Thin film deposition/Alcatel|Alcatel]])
! E-beam evaporation ([[Specific Process Knowledge/Thin film deposition/Temescal|Temescal]])
! E-beam evaporation ([[Specific Process Knowledge/Thin film deposition/Leybold|Leybold]])
! Thermal evaporation ([[Specific Process Knowledge/Thin film deposition/thermalevaporator|Thermal Evaporator]])
! Sputter deposition ([[Specific Process Knowledge/Thin film deposition/Lesker|Lesker]])
! Sputter deposition ([[Specific Process Knowledge/Thin film deposition/Cluster-based multi-chamber high vacuum sputtering deposition system|Sputter-system Metal-Oxide (PC1) and Sputter-system Metal-Nitride (PC3)]])
|-  
|-  
| Batch size
|-style="background:WhiteSmoke; color:black"
! General description
| E-beam deposition of Sn (line-of-sight)
| Thermal deposition of Sn (line-of-sight)
| Sputter deposition of Sn (some step coverage)
| Sputter deposition of Sn (pulsed DC, HiPIMS and substrate heating available)
 
|-
|-style="background:LightGrey; color:black"
!Pre-clean
|Ar ion  clean
|none
|none
|RF sputter cleaning
|-
|-style="background:WhiteSmoke; color:black"
!Layer thickness
| discuss with staff
1 nm to at least 100 nm
| discuss with staff
1 nm to at least 50 nm
| discuss with staff
| discuss with staff
1 nm to at least 50 nm
|-
|-style="background:LightGrey; color:black"
! Deposition rate
| discuss with staff (on the order of 1-5 Å/s)
| discuss with staff (on the order of 1-5 Å/s)
| discuss with staff
| discuss with staff (on the order of 1-2 Å/s)
|-
 
|-style="background:WhiteSmoke; color:black"
!Pre-clean
|Ar ion bombardment
|none
|none
|RF sputter cleaning
|-style="background:LightGrey; color:black"
! Batch size
|
*Up to 4x6" wafers or
*Up to 3x8" wafers or
*smaller pieces
|
*Up to 1x8" wafer or 1x6" wafer
*Up to 3x4" wafers
*smaller pieces
|
|
*Up to 1x4" wafers
*1x6" wafers or
*1x4" wafers or
*smaller pieces
*smaller pieces
|
|
*8x4" wafers or
*up to 10x6" wafers or
*5x6" wafers
*up to 10x4" wafers or
|-
*many smaller pieces
| Pre-clean
|RF Ar clean
|Ar ion bombartment
|-
| Layer thickness
|10Å to 1µm
|10Å to 1500Å
|-
| Deposition rate
|2Å/s to 15Å/s
|1Å/s to 5Å/s
|-
|-
|-style="background:WhiteSmoke; color:black"
!Allowed materials
|
* Almost any that does not outgas
*See also the [https://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=429 cross-contamination sheet]
|
* Almost any that do not degas. See also the [https://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=404 cross-contamination sheet]
|
* Almost any that do not degas. See also the [https://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=244 cross-contamination sheet]
|
*Almost any that does not degas at your intended substrate temperature. See cross contamination sheets for [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=441 PC1] and [https://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=442 PC3]
|-style="background:LightGrey; color:black"
! Comment
| Resulting films are rough
| Resulting films are very rough
| Resulting films are rough
| Resulting films are rough
|}
|}