Specific Process Knowledge/Thin film deposition/Si sputter in Wordentec: Difference between revisions
| (12 intermediate revisions by 4 users not shown) | |||
| Line 1: | Line 1: | ||
{{cc-nanolab}} | |||
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.labadviser.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Si_sputter_in_Wordentec click here]''' | '''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.labadviser.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Si_sputter_in_Wordentec click here]''' | ||
= | '''<p style="color:red;">The Wordentec has been decomissioned in 2025. These results are kept for reference.</p>''' | ||
Silicon | = Silicon sputtering in the Wordentec= | ||
Silicon can be sputter deposited in the [[Specific Process Knowledge/Thin film deposition/Wordentec|Wordentec]] as well as in the [[Specific Process Knowledge/Thin film deposition/Lesker|Sputter-System(Lesker)]] (details on sputtering Si in the Sputter-System Lesker [[Specific Process Knowledge/Thin film deposition/Deposition of Silicon/Si sputter in Sputter-System Lesker|here]]) and in the new [[Specific Process Knowledge/Thin film deposition/Cluster-based multi-chamber high vacuum sputtering deposition system|Cluster Lesker]] (results [[Specific Process Knowledge/Thin film deposition/Deposition of Silicon/Si sputter in Sputter-System Metal-Oxide(PC1)|here]] and [[Specific Process Knowledge/Thin film deposition/Deposition of Silicon/Si sputter in Sputter-System Metal-Oxide(PC3)|here]]). | |||
Listed below are tried parameters, that can be used during deposition. The process parameters in the table below can be used as started values, run a test process to be sure that you get the right thickness. | ==Parameters== | ||
Listed below are tried parameters, that can be used during Si deposition in the Wordentec. The process parameters in the table below can be used as started values, run a test process to be sure that you get the right thickness. | |||
'''Do not use the power more than 180 W without consulting staff''', since the Si target could break into a lot of small pieces. | '''Do not use the power more than 180 W without consulting staff''', since the Si target could break into a lot of small pieces. | ||
| Line 37: | Line 41: | ||
|- | |- | ||
|} | |} | ||
Latest revision as of 22:21, 20 June 2025
The content on this page, including all images and pictures, was created by DTU Nanolab staff, unless otherwise stated.
Feedback to this page: click here
The Wordentec has been decomissioned in 2025. These results are kept for reference.
Silicon sputtering in the Wordentec
Silicon can be sputter deposited in the Wordentec as well as in the Sputter-System(Lesker) (details on sputtering Si in the Sputter-System Lesker here) and in the new Cluster Lesker (results here and here).
Parameters
Listed below are tried parameters, that can be used during Si deposition in the Wordentec. The process parameters in the table below can be used as started values, run a test process to be sure that you get the right thickness.
Do not use the power more than 180 W without consulting staff, since the Si target could break into a lot of small pieces.
| Settings 1 | Settings 2 | |
|---|---|---|
| Process type | Sputtering | Sputtering |
| Power | 130W | 170W |
| Sputter pressure | 5*10-3 mbar | 1*10-2 mbar |
| Rate | About 0.7 Å/s | About 0.6 Å/s |