Specific Process Knowledge/Etch/Titanium Oxide: Difference between revisions
Appearance
No edit summary |
|||
| (13 intermediate revisions by 3 users not shown) | |||
| Line 1: | Line 1: | ||
Etch of Titanium oxide has been test in the ICP metal etcher. | '''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/Titanium_Oxide click here]''' | ||
<!-- Page reviewed 9/8-2022 jmli --> | |||
==Etch of Titanium oxide has been test in the ICP metal etcher. == | |||
*[[/ICP metal|Titanium Oxide etch using ICP metal]] | *[[/ICP metal|Titanium Oxide etch using ICP metal]] | ||
*Titanium Oxide etch using BHF | |||
==Comparison of Titanium Oxide (ALD) etch Methods == | |||
{|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" | |||
|- | |||
|- | |||
|-style="background:silver; color:black" | |||
! | |||
!BHF | |||
!ICP Metal Etcher | |||
|- | |||
|- | |||
|-style="background:WhiteSmoke; color:black" | |||
!Generel description | |||
|Wet etch of TiO2 (ALD) | |||
|Dry etch of TiO2 | |||
|- | |||
|- | |||
|-style="background:LightGrey; color:black" | |||
!Etch rate range | |||
|2,5 nm/min | |||
| | |||
*It has not been explored | |||
*current recipe ~8 nm/min | |||
|- | |||
|- | |||
|-style="background:WhiteSmoke; color:black" | |||
!Etch profile | |||
| | |||
*Isotropic | |||
| | |||
*Anisotropic | |||
|- | |||
|- | |||
|-style="background:LightGrey; color:black" | |||
!Substrate size | |||
| | |||
* | |||
*Any size (in beaker) | |||
| | |||
*Samples < 150 mm wafers on carrier | |||
*one 150 mm wafer at a time | |||
|- | |||
|- | |||
|-style="background:WhiteSmoke; color:black" | |||
!'''Allowed materials''' | |||
|In beaker: | |||
*Any material | |||
| | |||
*silicon, silicon oxides and nitrides | |||
*Al, Cr, Ti (incl. oxides and nitrides) | |||
*Ta, W, Nb (incl. oxides and nitrides) | |||
|- | |||
|} | |||
Latest revision as of 15:23, 4 September 2025
Feedback to this page: click here
Etch of Titanium oxide has been test in the ICP metal etcher.
- Titanium Oxide etch using ICP metal
- Titanium Oxide etch using BHF
Comparison of Titanium Oxide (ALD) etch Methods
| BHF | ICP Metal Etcher | |
|---|---|---|
| Generel description | Wet etch of TiO2 (ALD) | Dry etch of TiO2 |
| Etch rate range | 2,5 nm/min |
|
| Etch profile |
|
|
| Substrate size |
|
|
| Allowed materials | In beaker:
|
|