Jump to content

Specific Process Knowledge/Thin film deposition/Electroplating-Ni: Difference between revisions

Jmli (talk | contribs)
No edit summary
Mmat (talk | contribs)
 
(13 intermediate revisions by 5 users not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:fabricationSupport@Nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Electroplating-Ni click here]'''
'''<p style="color:red;">The Electroplater Technotrans microform.200 has been decomissioned. For electroplating, please contact DTU Mechanical Engineering.</p>'''


[[Category: Equipment|Thin film Electroplating Ni]]
[[Category: Equipment|Thin film Electroplating Ni]]
[[Category: Thin Film Deposition|Electroplating Ni]]
[[Category: Thin Film Deposition|Electroplating Ni]]


== Technotrans microform.200 ==
= Technotrans microform.200=


[[image:Electroplater-D3.jpg|200x200px|right|thumb|Electroplating-Ni positioned in cleanroom D-3]]
[[image:Electroplater-D3.jpg|200x200px|right|thumb|Electroplating-Ni positioned in cleanroom D-3]]
Line 26: Line 26:
Uniformity across a 4" wafer is around 5% for the standard processes (the edge being slightly thicker than the center of the sample). Running at high current densities will deposit a nickel layer that is quite soft. Decreasing current density will increase tensile strength of the deposited nickel.
Uniformity across a 4" wafer is around 5% for the standard processes (the edge being slightly thicker than the center of the sample). Running at high current densities will deposit a nickel layer that is quite soft. Decreasing current density will increase tensile strength of the deposited nickel.


'''The user manual(s), quality control procedure(s) and results, user APV(s), technical information and contact information can be found in LabManager:'''
<!-- remember to remove the type of documents that are not present -->
<!-- give the link to the equipment info page in LabManager: -->
[http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=274 Electroplating-Ni Info on LabManager]
== Process information ==
*[[Specific Process Knowledge/Thin film deposition/Deposition of Nickel/Electroplating of nickel|Description of standard processes]]


==Equipment performance and process related parameters==
==Equipment performance and process related parameters==
Line 93: Line 81:
|style="background:LightGrey; color:black"|Thickness
|style="background:LightGrey; color:black"|Thickness
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
0 - 1400 µm
~20 - 1000 µm


|-
|-
Line 109: Line 97:
|style="background:LightGrey; color:black"|pH
|style="background:LightGrey; color:black"|pH
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
~3,70 (maintained automatically)
~3,65 (maintained automatically)
   
   
|-
|-
Line 124: Line 112:
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Most materials '''except copper and cobalt'''.
*Most materials '''except copper and cobalt'''.
*Ask Danchip for details.
*Ask Nanolab for details.
|-  
|-  
|}
|}
== DTU Nanolab Standard Programs for Electroplating of Nickel ==
Three different standard programs have been made by DTU Nanolab. They have all been made to fabricate nickel shims for use in the polymer injection molding machine at DTU Nanolab. For this purpose a nickel thickness of around 340-360 µm is optimal. By experimentation it has been found that the required charge for this sample thickness is 18,3 Ah. The only difference between the different standard programs is the time required for depositing the nickel. The three different standard programs deposit the ~350 µm of nickel in about 4, 6 or 12 hours respectively.
The following figure shows the current profile during the first 2 hours of the programs:
[[Image:CurrentProfiles2019.png|center|Current profiles of standard programs]]
As can be seen from the illustration the first 30 minutes of all standard processes are identical. All processes use a slow ramping of the current. This is to make sure that some material is deposited which can conduct a higher current. Starting a plating process at several amperes is very likely to damage the sample (and possibly the sample holder) because the seed metal layer (usually 50-120 nm thick) cannot support such high currents.
The Standard programs are named using the following convention: '''DCHimmXX.X-YY''' where '''DCH''' indicates it's a process developed by Nanolab, '''imm''' that is a process developed for producing samples for the '''i'''njection '''m'''olding '''m'''achine, '''XX.X''' denotes the charge in Ah (Ampere-hours) and '''YY''' denotes the approximate process time in hours.
<br clear="all" />
==Comparison of standard processes==
{|border="1" cellspacing="1" cellpadding="3" style="text-align:left;"
|-
|-
|-style="background:silver; color:black"
!
!DCHimm18.3-04
!DCHimm18.3-06
!DCHimm18.3-12
|-
|-
|-style="background:WhiteSmoke; color:black"
!Charge [Ah]
|18,3
|18,3
|18,3
|-
|-
|-style="background:WhiteSmoke; color:black"
!Expected nickel thickness
|350 µm
|350 µm
|350 µm
|-
|-
|-style="background:LightGrey; color:black"
!Maximum current [A]
|
5,5
|
3,5
|
1,5
|-
|-
|-style="background:WhiteSmoke; color:black"
!Process time [hh:mm:ss]
|
04:10:55
|
06:12:52
|
12:28:01
|-
|-
|-style="background:LightGrey; color:black"
!Process comments
|
A fast program that allows one to produce two samples in a normal working day. Usually works fine for rapid prototyping.
|
A compromise between desired material properties (hardness, ductility, roughness) and process time. Will result in a sample that will be useful for most standard injection molding processes.
|
A slower process that in return results in lower roughness and stronger mechanical properties. A good choice for shims that will be used with 'harsh' injection molding parameters (high temperatures and high pressures).
|-
|}
<br clear="all" />