'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Aluminum_Oxide/Al2O3_Etch_using_HF click here]''' | '''Unless anything else is stated, everything on this page, text and pictures are made by DTU Nanolab.''' | ||
'''All links to Kemibrug (SDS) and Labmanager Including APV and QC requires login.''' | |||
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/Aluminum_Oxide/Al2O3_Etch_using_HF click here]''' | |||
| Line 6: | Line 10: | ||
=== Experiment and results === | === Experiment and results === | ||
Si samples with about 100 nm of [[Specific_Process_Knowledge/Thin_film_deposition/ALD_Picosun_R200|ALD]] deposited Al<sub>2</sub>O<sub>3</sub> (1000 cycles at 300<sup>o</sup>C) has been etched in different HF concentrations. After the etching, the thickness of the Al<sub>2</sub>O<sub>3</sub> layer has been measured, and the thickness as function of time has been plotted as shown in the graph below. | Si samples with about 100 nm of [[Specific_Process_Knowledge/Thin_film_deposition/ALD_Picosun_R200|ALD]] deposited Al<sub>2</sub>O<sub>3</sub> (1000 cycles at 300<sup>o</sup>C) has been etched in different HF concentrations. After the etching, the thickness of the Al<sub>2</sub>O<sub>3</sub> layer has been measured using [[Specific_Process_Knowledge/Characterization/Optical_characterization#Ellipsometer|Ellipsometer VASE]], and the thickness as function of time has been plotted as shown in the graph below. | ||
<gallery caption=" | <gallery caption="" widths="600px" heights="500px" perrow="1"> | ||
image:Al2O3_HF_20190826.png| | image:Al2O3_HF_20190826.png| Different etching rates for different HF concentrations. | ||
</gallery> | </gallery> | ||
| Line 15: | Line 19: | ||
The etch rates: | The etch rates: | ||
<ul> | <ul> | ||
<li> 5% HF | <li><p>5% HF → <b>1.74 nm/s</b></p></li> | ||
<li> 1vol. H<sub>2</sub>O : 1vol. 5% HF 1.05 nm/s </li> | <li><p> 1vol. H<sub>2</sub>O : 1vol. 5% HF → <b>1.05 nm/s</b></p></li> | ||
<li> 2vol. H<sub>2</sub>O : 1vol. 5% HF 0. | <li><p> 2vol. H<sub>2</sub>O : 1vol. 5% HF → <b>0.72 nm/s</b></p></li> | ||
</ul> | </ul> | ||
Be aware of that the 5% HF etches quite fast | Be aware of that the 5% HF etches quite fast. Actually, so fast that it can be tricky to control. Taking the sample out of the solution and placing it in a bigger water container to rinse, resulting a time delay due to the movement and the etch continues. It means the handling things around the fumehood can be a source of errors in this case. | ||
''Evgeniy Shkondin, DTU Nanolab, June 2019'' | ''Evgeniy Shkondin, DTU Nanolab, June 2019'' | ||
=== Photoresist adhesion === | |||
Experiments in April 2025 as shown bad adhesion of AZ 5214E on Al2O3. Total delamination occurred in less than 120 seconds on 50nm and 100nm of Al2O3 deposited using ALD. | |||
Thus wetetch is unsuitable to structure an Al2O3 for use as hard-mask for dryetching. | |||
<br> | |||
Systematic studies have not yet been done as of April 2025. | |||
<br> | |||
Following parameters were tested: | |||
{| class="wikitable" | |||
|+ Process parameters | |||
|- | |||
!style="max-width:7em;"| ALD Parameters | |||
|| | |||
* Cycles: 500 and 1000 | |||
* Temperature: 200°C | |||
* TMA pulse: 0.1s | |||
* H2O pulse: 0.1s | |||
|- | |||
!style="max-width:7em;"| Lithography parameters | |||
|| | |||
* Pretreatment: HMDS | |||
* Resist type: AZ 5214E | |||
* Resist thickness: 1.5µm | |||
* Exposure parameters: | |||
** Tool: MLA3 | |||
** Dose: 100 mJ/cm2 | |||
** Defocus: 1 | |||
** Mode: Fast | |||
* Development: TMAH, SP60 | |||
* Post treatment: Hardbake 120s@120C | |||
|} | |||
''Jesper Pan, DTU Nanolab, April 2025'' | |||