Specific Process Knowledge/Etch/ICP Metal Etcher/silicon/isotropic: Difference between revisions
Appearance
No edit summary |
|||
| (5 intermediate revisions by 2 users not shown) | |||
| Line 1: | Line 1: | ||
= Isotropic etching in silicon on the ICP Metal Etch = | = Isotropic etching in silicon on the ICP Metal Etch = | ||
<!--Checked for updates on 11/2-2019 - ok/jmli --> | <!--Checked for updates on 11/2-2019 - ok/jmli --> | ||
<!--Checked for updates on 24/8-2021. ok/ jmli--> | |||
<!--Checked for updates on 4/4-2025 - ok/jmli --> | |||
{| border="1" cellpadding="0" cellspacing="0" style="text-align:center;" | {| border="1" cellpadding="0" cellspacing="0" style="text-align:center;" | ||
| Line 35: | Line 36: | ||
| 20 <!--Temperature --> | | 20 <!--Temperature --> | ||
| - <!--Process time (needed if ramping is enabled) --> | | - <!--Process time (needed if ramping is enabled) --> | ||
| | | 10 <!--Pressure --> | ||
| - <!--Process chamber setup --> | | - <!--Process chamber setup --> | ||
| 90 <!--SF6 flow --> | | 90 <!--SF6 flow --> | ||
| Line 50: | Line 51: | ||
| 3 <!--Platen power --> | | 3 <!--Platen power --> | ||
| [[Specific Process Knowledge/Etch/ICP Metal Etcher/silicon/isotropic/isoslow1|'''Click HERE!''' ]] <!-- link processes --> | | [[Specific Process Knowledge/Etch/ICP Metal Etcher/silicon/isotropic/isoslow1|'''Click HERE!''' ]] <!-- link processes --> | ||
| | | Note: Lior Shiv got very high etch rate for this recipe >1.5µm/min 2019-07-12 <!--Keywords --> | ||
|- | |- | ||
|- | |||
! no name, tested by Lior Shiv@Capres 2019-07-12 <!--Recipe Name --> | |||
| A <!--Step --> | |||
| 20 <!--Temperature --> | |||
| - <!--Process time (needed if ramping is enabled) --> | |||
| 10 <!--Pressure --> | |||
| - <!--Process chamber setup --> | |||
| 90 <!--SF6 flow --> | |||
| 0 <!--O2 flow --> | |||
| 0 <!--C4F8 flow --> | |||
| 0 <!--Ar flow --> | |||
| 0 <!--CF4 flow --> | |||
| 0 <!--H2 flow --> | |||
| 0 <!--CH4 flow --> | |||
| 0 <!--BCl3 flow --> | |||
| 0 <!--Cl2 flow --> | |||
| 0 <!--HBr flow --> | |||
| 150 <!--Coil power --> | |||
| 3 <!--Platen power --> | |||
| <!-- link processes --> | |||
| About 10% load, etch rate around 400nm/min <!--Keywords --> | |||
|- | |||
|} | |} | ||
Latest revision as of 08:34, 4 April 2025
Isotropic etching in silicon on the ICP Metal Etch
| Recipe | Step | Temp. | Time | Pres. | Hardware | Gasses | RF powers | Observations | |||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| SF6 | O2 | C4F8 | Ar | CF4 | H2 | CH4 | BCl3 | Cl2 | HBr | Coil | Platen | SEM images of different runs | Keywords | ||||||
| isoslow1 | A | 20 | - | 10 | - | 90 | 0 | 0 | 0 | 0 | 0 | 0 | 0 | 0 | 0 | 400 | 3 | Click HERE! | Note: Lior Shiv got very high etch rate for this recipe >1.5µm/min 2019-07-12 |
| no name, tested by Lior Shiv@Capres 2019-07-12 | A | 20 | - | 10 | - | 90 | 0 | 0 | 0 | 0 | 0 | 0 | 0 | 0 | 0 | 150 | 3 | About 10% load, etch rate around 400nm/min | |