LabAdviser/Technology Research/Fabrication of Hyperbolic Metamaterials using Atomic Layer Deposition/TIO ALU Gratings Procces flow: Difference between revisions

From LabAdviser
Eves (talk | contribs)
Eves (talk | contribs)
No edit summary
 
(3 intermediate revisions by the same user not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/LabAdviser/Technology_Research/Fabrication_of_Hyperbolic_Metamaterials_using_Atomic_Layer_Deposition/TIO_ALU_Gratings_Procces_flow click here]'''
<i>This page is written by <b>Evgeniy Shkondin @DTU Nanolab</b> if nothing else is stated. <br>
All images and photos on this page belongs to <b>DTU Nanolab</b> and <b>DTU Electro</b> (previous DTU Fotonik).<br>
The fabrication and characterization described below were conducted in <b>2013-2016 by Evgeniy Shkondin, DTU Nanolab</b>.<br></i>
====Procces flow description====
====Procces flow description====


All samples were prepared and characterized in a class 100 cleanroom. Si (100) wafers of 150 mm were used as a substrate. The main steps in the gratings manufacturing are shown in a figure below. First, the silicone trenches were realized by deep reactive ion etching (DRIE). Then, the trenches were ALD coated. After the selective removal of the top parts, the silicon core between ALD coatings was etched away during the last step. The final structure represents the highly anisotropic vertical grating. Each fabrication step was carefully evaluated using cross-sectional scanning electron microscopy (SEM) imaging.
All samples were prepared and characterized in a class 100 cleanroom. Si (100) wafers of 150 mm were used as a substrate. The main steps in the gratings manufacturing are shown in a figure below. First, the silicon trenches were realized by deep reactive ion etching (DRIE). Then, the trenches were ALD coated. After the selective removal of the top parts, the silicon core between ALD coatings was etched away during the last step. The final structure represents the highly anisotropic vertical grating. Each fabrication step was carefully inspected using cross-sectional scanning electron microscopy (SEM) imaging.





Latest revision as of 13:43, 2 February 2023

Feedback to this page: click here

This page is written by Evgeniy Shkondin @DTU Nanolab if nothing else is stated.
All images and photos on this page belongs to DTU Nanolab and DTU Electro (previous DTU Fotonik).
The fabrication and characterization described below were conducted in 2013-2016 by Evgeniy Shkondin, DTU Nanolab.

Procces flow description

All samples were prepared and characterized in a class 100 cleanroom. Si (100) wafers of 150 mm were used as a substrate. The main steps in the gratings manufacturing are shown in a figure below. First, the silicon trenches were realized by deep reactive ion etching (DRIE). Then, the trenches were ALD coated. After the selective removal of the top parts, the silicon core between ALD coatings was etched away during the last step. The final structure represents the highly anisotropic vertical grating. Each fabrication step was carefully inspected using cross-sectional scanning electron microscopy (SEM) imaging.


Process flow

Description of steps for fabrication of TiO2 and AL2O3 nanogratings.

Step Description LabAdviser link Image showing the step
1.1 Plasma surface treatment To ensure clean surface, the 100 mm Si wafer is treated by O2/N2 plasma. (Optional step) Plasma Asher 2
1.2 DUV Resist patterning DUV DUV Stepper Lithography.
1.3 Deep reactive ion etching (DRIE) DRIE; Recipe: PolySOI10 DRIE Pegasus.
1.4 Plasma surface treatment To ensure that remainings of DUV resist are gone, samples are treated by O2/N2 plasma. (Optional step) Plasma Asher 2.
1.5 Scanning Electron Microscopy inspection By cleaving the sample it is possible to inspect DRIE etched Si trenches in cross-sectional mode

SEM Supra 1
SEM Supra 2
SEM Supra 3

1.6 Atomic Layer Deposition of either Al2O3 or TiO2 Deposition carried at 150C.Thickness is 90 nm. Equipment used: ALD Picosun R200. Standard recipes used: Al2O3T and TiO2T .
1.7 Scanning Electron Microscopy inspection By cleaving the sample it is possible to inspect ALD coatings deposited on Si trenches in cross-sectional mode

SEM Supra 1
SEM Supra 2
SEM Supra 3

1.8 Opening of deposited Al2O3 or TiO2 top layers. Etching happens using ICP Metal etcher with Cl2/BCl3 process gasses. Equipment used: Metal ICP Etcher.
1.9 Scanning Electron Microscopy inspection By cleaving the sample it is possible to inspect ICP etcher results Si trenches in cross-sectional mode

SEM Supra 1
SEM Supra 2
SEM Supra 3

1.10 Selective etch of Si between ALD Al2O3 or TiO2 coatings. Si etching proceeds using ICP Metal etcher with isotropic process based on SFf process gas. Equipment used: Metal ICP Etcher.
1.11 Scanning Electron Microscopy inspection of fabricated structure. Proof of final result.

SEM Supra 1
SEM Supra 2
SEM Supra 3

1.12 Ion beam etching. (Optional) Additional shape of the top part. 20 mijn etch using recipe "Ti acceptance" there the stage shoud be placed to 0o degree. SEM cross section is used for inspection IBE/IBSD Ionfab 300