Specific Process Knowledge/Etch/DRIE-Pegasus/DUVetch: Difference between revisions
Appearance
No edit summary |
|||
| (4 intermediate revisions by the same user not shown) | |||
| Line 1: | Line 1: | ||
'''Feedback to this page''': '''[mailto:labadviser@ | '''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/DRIE-Pegasus/DUVetch click here]''' | ||
<!--Checked for updates on 14/5-2018 - ok/jmli --> | <!--Checked for updates on 14/5-2018 - ok/jmli --> | ||
<!--Checked for updates on 24/8-2021. ok/ jmli--> | |||
<!--Checked for updates on 4/4-2025 - ok/jmli --> | |||
== Etch processes designed for stepper resists == | == Etch processes designed for stepper resists == | ||
| Line 151: | Line 153: | ||
= | = With units = | ||
{| border="2" cellpadding="2" cellspacing="1" style="text-align:center;" | {| border="2" cellpadding="2" cellspacing="1" style="text-align:center;" | ||
| Line 250: | Line 252: | ||
|+ '''Process parameters''' | |+ '''Process parameters''' | ||
|- | |- | ||
! rowspan=" | ! rowspan="3" width="100"| Recipe | ||
! rowspan=" | ! rowspan="3" width="20"| Step | ||
! rowspan="2" width="20"| Temp. | ! rowspan="2" width="20"| Temp. | ||
! colspan="6" | Deposition step | ! colspan="6" | Deposition step | ||
| Line 271: | Line 273: | ||
! width="40" | Coil | ! width="40" | Coil | ||
| [[Specific Process Knowledge/Etch/DRIE-Pegasus/Parameters#Platen power|Platen]] | | [[Specific Process Knowledge/Etch/DRIE-Pegasus/Parameters#Platen power|Platen]] | ||
| [[Specific Process Knowledge/Etch/DRIE-Pegasus/Parameters#Hardware | HW]] | | rowspan="2" | [[Specific Process Knowledge/Etch/DRIE-Pegasus/Parameters#Hardware | HW]] | ||
! width="40" | Runs | ! width="40" rowspan="2" | Runs | ||
! width="300" | Key words | ! width="300" rowspan="2" | Key words | ||
|- | |||
| degs | |||
| s | |||
| mt | |||
| sccm | |||
| sccm | |||
| sccm | |||
| W | |||
| s | |||
| mt | |||
| sccm | |||
| sccm | |||
| sccm | |||
| W | |||
| W | |||
|- | |- | ||
! polySOI-10 <!-- recipe name --> | ! polySOI-10 <!-- recipe name --> | ||
Latest revision as of 08:37, 4 April 2025
Feedback to this page: click here
Etch processes designed for stepper resists
The stepper produces features down to 200 nm. Here, etch processes especially designed for stepper patterns and resists are described. We intend to develop them continuously so keep an eye on this page. The best ones so far are:
| Recipe | Step | Temp. | Deposition step | Etch step | Process | ||||||||||||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Time | Pressure | C4F8 | SF6 | O2 | Coil | Time | Pressure | C4F8 | SF6 | O2 | Coil | Platen | HW | Runs | Keywords | ||||||||||
| B | M | B | M | B | M | B | M | B | M | B | M | B | M | ||||||||||||
| NBoost04 | A | 20 | 2.8 | 5 | 60 | 0 | 0 | 500 | 1.5 | 3.5 | 30% | 5 | 0 | 20 | 100 | 100 | 0 | 0 | 500 | 500 | 50 | 10 | LF+B100 | 2 | VERY nice: scallops, straight sidewalls |
| Recipe | Step | Temp. | Deposition step | Etch step | Process observations | |||||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Time | Pressure | C4F8 | SF6 | O2 | Coil | Time | Pressure | C4F8 | SF6 | O2 | Coil | Platen | HW | Runs | Key words | |||
| polySOI-10 | etch | 20 | 2.5 | 10 | 50 | 0 | 0 | 600 | 5 | 10 | 20 | 60 | 5 | 400 | 40 | - | 5 | very nice, blurred scallops |
| polySOI-10a | etch | 20 | 2.5 | 10 | 50 | 0 | 0 | 600 | 5 | 10 | 10 | 70 | 5 | 400 | 40 | - | 200+ | Works only with limited open area - probably less than 20 %, very stable, excellent and extensive track record |
With units
| Recipe | Step | Temp. | Deposition step | Etch step | Process | ||||||||||||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Time | Pressure | C4F8 | SF6 | O2 | Coil | Time | Pressure | C4F8 | SF6 | O2 | Coil | Platen | HW | Runs | Keywords | ||||||||||
| B | M | B | M | B | M | B | M | B | M | B | M | B | M | ||||||||||||
| degs | s | mt | sccm | sccm | sccm | W | s | s | % | mt | sccm | sccm | sccm | sccm | sccm | sccm | W | W | W | W | |||||
| NBoost04 | A | 20 | 2.8 | 5 | 60 | 0 | 0 | 500 | 1.5 | 3.5 | 30% | 5 | 0 | 20 | 100 | 100 | 0 | 0 | 500 | 500 | 50 | 10 | LF+B100 | 2 | VERY nice: scallops, straight sidewalls |
| Recipe | Step | Temp. | Deposition step | Etch step | Process observations | |||||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Time | Pressure | C4F8 | SF6 | O2 | Coil | Time | Pressure | C4F8 | SF6 | O2 | Coil | Platen | HW | Runs | Key words | |||
| degs | s | mt | sccm | sccm | sccm | W | s | mt | sccm | sccm | sccm | W | W | |||||
| polySOI-10 | etch | 20 | 2.5 | 10 | 50 | 0 | 0 | 600 | 5 | 10 | 20 | 60 | 5 | 400 | 40 | - | 5 | very nice, blurred scallops |
| polySOI-10a | etch | 20 | 2.5 | 10 | 50 | 0 | 0 | 600 | 5 | 10 | 10 | 70 | 5 | 400 | 40 | - | 200+ | Works only with limited open area - probably less than 20 %, very stable, excellent and extensive track record |