<!--Checked for updates on 21/10-2025. ok/ jmli-->
=Processing of high resolution scanned spectra =
=Processing of high resolution scanned spectra =


Line 52: Line 55:


== The Ti2p peak ==
== The Ti2p peak ==
The titanium Ti2p peak is notoriously difficult to fit. From [[Specific Process Knowledge/Characterization/XPS/Processing/XPSknowledgeview |XPS Knowledge view]] we have:
The titanium Ti2p peak is notoriously difficult to fit. Let us first look for some clues in [[Specific Process Knowledge/Characterization/XPS/Processing/XPSknowledgeview |XPS Knowledge view]]. The section below is a copy of the content in XPS Knowledge View (Avantage version 5.986).
 
=== XPS Knowledge on the fitting of the Ti2p peak ===


'''''Binding energies of common chemical states'''''
'''''Binding energies of common chemical states'''''
Line 61: Line 66:
| ''Ti metal'' || ''454.1''
| ''Ti metal'' || ''454.1''
|-
|-
| ''TiN'' || 545.9
| ''TiN'' || 454.9
|-
|-
| ''TiO<sub>2</sub>'' || ''458.5''
| ''TiO<sub>2</sub>'' || ''458.5''
Line 87: Line 92:
** ''Sub-oxides and/or metal may be formed during sputtering of the oxide.''
** ''Sub-oxides and/or metal may be formed during sputtering of the oxide.''


=== The fitting of the Ti2p peak ===


 
'''Please note that clicking on any of the two spectra above when using XPS Knowledge View in Avantage will generate a new processing grid with this particular set of data, peak table etc. It may be quite convenient to investigate what constraints have been added - obviously also for any other element.'''
'''Please note that clicking on any of the two spectra above when using XPS Knowledge View will generate a new processing grid in Avantage with this particular set of data, peak table etc. It may be quite convenient to investigate what constraints have been added - obviously also for any other element.'''


The only challenge we are missing from this cocktail of asymmetric peak shapes, differences in spin-orbit splitting, reduction of fully oxidized Ti2p to sub-oxides and satellite features is the presence of TiN.
The only challenge we are missing from this cocktail of asymmetric peak shapes, differences in spin-orbit splitting, reduction of fully oxidized Ti2p to sub-oxides and satellite features is the presence of TiN.


First, let us find some reasonable parameters for the Ti2p metallic peak. For that purpose, we analyse an old data set acquired on pure Ti.
First, let us find some reasonable parameters for the Ti2p metallic peak. For that purpose, we analyse an old data set acquired on pure Ti.
[[File:Ti 2p highres 1.jpg|700px]]