Specific Process Knowledge/Back-end processing/Laser Micromachining Tool/fluence: Difference between revisions
Appearance
mNo edit summary |
|||
| (3 intermediate revisions by one other user not shown) | |||
| Line 1: | Line 1: | ||
{{cc-nanolab}} | |||
== Fluence definition == | == Fluence definition == | ||
| Line 11: | Line 14: | ||
Where <math>\overline{P}</math> (average power) is measured with the laser sensor power measurement (see [http://labmanager.danchip.dtu.dk/d4Show.php?id=2885&mach=309|laser manual],section 5.3) and the repetion rate (<math>f</math>) is set in the parameter file under " laser frequency". | Where <math>\overline{P}</math> (average power) is measured with the laser sensor power measurement (see [http://labmanager.danchip.dtu.dk/d4Show.php?id=2885&mach=309|laser manual],section 5.3) and the repetion rate (<math>f</math>) is set in the parameter file under " laser frequency". | ||
The fluence is therefore determinated as such : | The fluence is therefore determinated as such: | ||
Latest revision as of 18:04, 27 May 2025
The content on this page, including all images and pictures, was created by DTU Nanolab staff, unless otherwise stated.
Fluence definition
The fluence produces by a laser is, by definition, the energy delivered by a laser pulse () per surface unit () and it is given in J/cm2.
The function is defined as:
Where (average power) is measured with the laser sensor power measurement (see manual,section 5.3) and the repetion rate () is set in the parameter file under " laser frequency".
The fluence is therefore determinated as such:
The area () can be determinate with the theoretical min spot diameter (1/e2), available here
Fluence results measurement
The results below have been calculated with the theoretical spot size provided by 3D Micromac.