Specific Process Knowledge/Etch/DRIE-Pegasus: Difference between revisions
No edit summary |
|||
| (95 intermediate revisions by 3 users not shown) | |||
| Line 1: | Line 1: | ||
'''Feedback to this page: | '''Feedback to this page: | ||
[mailto:labadviser@ | [mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/DRIE-Pegasus click here]''' | ||
[[Category: Equipment |Etch DRIE]] | [[Category: Equipment |Etch DRIE]] | ||
[[Category: Etch (Dry) Equipment|DRIE]] | [[Category: Etch (Dry) Equipment|DRIE]] | ||
= The DRIE Pegasus tools at DTU Nanolab = | |||
{{Template:Author-jmli1}} | |||
<!--Checked for updates on 2/02-2023 - ok/jmli --> | |||
<!--Checked for updates on 21/10-2025 - ok/jmli --> | |||
In 2010 DTU Nanolab acquired DRIE-Pegasus 1. As a state-of-the-art etch tool with excellent performance and great flexibility, it grew immensely popular and by 2015 it was apparent that we needed yet another tool to cope with the demand. Therefore, in 2016 Pegasus 2 was acquired from a closed-down lab and installed next to Pegasus 1. | |||
Looking to expand our dry etching capabilities in 2017 we got an irresistible offer on a twin Pegasus system with cassette to cassette vacuum robot from a commercial fab. The twin Pegasus system (called Pegasus 3 and 4) is installed at the old cluster 2 location in cleanroom C1 and will run only 6" wafers. Pegasus 3 is the 6" silicon etch work horse and Pegasus 4 is converted (adding extra process gases) into a 6" dielectric etch tool that will supplement/replace the AOE. | |||
This page was originally intended as a regular one-machine page (the Pegasus 1 page). However, as of 2018 with several tools, the page will serve as common page for all of our Pegasi with subpages for each tool. | |||
{| | {| | ||
| [[ | |width="100"| [[file:DRIE-Pegasus.jpg |100px|frameless]] | ||
| | | width="200"| [[file:Pegasus 2 operator.jpg |204px|frameless]] | ||
| width="275"|[[file:Peg3and4 front 2.JPG |292px|frameless]] | |||
| align="center" | DRIE- | |- | ||
| align="center" | The DRIE-Pegasus 1 load lock and cassette loader in the DTU Nanolab cleanroom A-1. {{photo1}} | |||
| align="center" | The DRIE-Pegasus 2 operator station and load lock in the DTU Nanolab cleanroom A-1. {{photo1}} | |||
| align="center" | The DRIE-Pegasus3 and DRIE-Pegasus4 operator station and cassette loading stations. {{photo1}} | |||
|- | |- | ||
|} | |} | ||
== The Bosch process == | == The Bosch process == | ||
The DRIE Pegasus tools are state-of-art silicon dry etchers that offer outstanding performance in terms of etch rate, uniformity etc. They use the so-called Bosch process to achieve excellent control of the etched features. Click [[Specific_Process_Knowledge/Etch/DRIE-Pegasus/System-description|'''HERE''']] | The DRIE Pegasus tools are state-of-art silicon dry etchers that offer outstanding performance in terms of etch rate, uniformity etc. They use the so-called Bosch process to achieve excellent control of the etched features. Click [[Specific_Process_Knowledge/Etch/DRIE-Pegasus/System-description|'''HERE''']] to access the top of the page. The contents are: | ||
# [[Specific_Process_Knowledge/Etch/DRIE-Pegasus/System-description#Description_of_the_Bosch_process_at_the_DRIE-Pegasus| Description of the Bosch process ]] | |||
# [[Specific_Process_Knowledge/Etch/DRIE-Pegasus/System-description#Processing_options_on_the_Pegasus | Processing options on the Pegasus ]] | |||
# [[Specific_Process_Knowledge/Etch/DRIE-Pegasus/System-description#Modification_of_the_showerhead | Modification of the showerhead ]] | |||
# [[Specific_Process_Knowledge/Etch/DRIE-Pegasus/System-description#RF_Matching | RF matching ]] | |||
## [[Specific_Process_Knowledge/Etch/DRIE-Pegasus/System-description#RF_matching_in_general | RF matching in general ]] | |||
## [[Specific_Process_Knowledge/Etch/DRIE-Pegasus/System-description#Why_RF_matching_is_extremely_important_in_the_Bosch_process | Why RF matching is extremely important in the Bosch process ]] | |||
# [[Specific Process Knowledge/Etch/DRIE-Pegasus/picoscope|Picoscope process monitoring]] | |||
As of 2017, completing the [[LabAdviser/Courses/TPT_Dry_Etch| Dry Etch TPT course]] is mandatory for all new users. On the TPT web page you will find a version of the latest lecture slides - here you will find information as well. | |||
== Links to the individual pages for the Pegasi == | == Links to the individual pages for the Pegasi == | ||
| Line 30: | Line 42: | ||
* [[Specific_Process_Knowledge/Etch/DRIE-Pegasus/Pegasus-1|DRIE-Pegasus 1]] | * [[Specific_Process_Knowledge/Etch/DRIE-Pegasus/Pegasus-1|DRIE-Pegasus 1]] | ||
* [[Specific_Process_Knowledge/Etch/DRIE-Pegasus/Pegasus-2|DRIE-Pegasus 2]] | * [[Specific_Process_Knowledge/Etch/DRIE-Pegasus/Pegasus-2|DRIE-Pegasus 2]] | ||
* [[Specific_Process_Knowledge/Etch/DRIE-Pegasus/Pegasus-3|DRIE-Pegasus 3 | * [[Specific_Process_Knowledge/Etch/DRIE-Pegasus/Pegasus-3|DRIE-Pegasus 3]] | ||
* [[Specific_Process_Knowledge/Etch/DRIE-Pegasus/Pegasus-4|DRIE-Pegasus 4 | * [[Specific_Process_Knowledge/Etch/DRIE-Pegasus/Pegasus-4|DRIE-Pegasus 4]] | ||
==Equipment performance and process related parameters== | ==Equipment performance and process related parameters== | ||
{| border="2" cellspacing="0" cellpadding=" | {| border="2" cellspacing="0" cellpadding="1" | ||
!colspan="2" border="none" style="background:silver; color:black;" align="center"|Equipment | !colspan="2" border="none" style="background:silver; color:black;" align="center"|Equipment | ||
|style="background:silver; color:black" width="250" |[[Specific Process Knowledge/Etch/DRIE-Pegasus/Pegasus-1| '''DRIE-Pegasus 1''']] | |style="background:silver; color:black" width="250" align ="center" |[[Specific Process Knowledge/Etch/DRIE-Pegasus/Pegasus-1| '''DRIE-Pegasus 1''']] | ||
|style="background:silver; color:black" width="250" |[[Specific Process Knowledge/Etch/DRIE-Pegasus/Pegasus-2| '''DRIE-Pegasus 2''']] | |style="background:silver; color:black" width="250" align ="center" |[[Specific Process Knowledge/Etch/DRIE-Pegasus/Pegasus-2| '''DRIE-Pegasus 2''']] | ||
|style="background:silver; color:black" width="250" |[[Specific Process Knowledge/Etch/DRIE-Pegasus/Pegasus-3| '''DRIE-Pegasus 3''']] | |style="background:silver; color:black" width="250" align ="center" |[[Specific Process Knowledge/Etch/DRIE-Pegasus/Pegasus-3| '''DRIE-Pegasus 3''']] | ||
|style="background:silver; color:black" width="250" |[[Specific Process Knowledge/Etch/DRIE-Pegasus/Pegasus-4| '''DRIE-Pegasus 4''']] | |style="background:silver; color:black" width="250" align ="center" |[[Specific Process Knowledge/Etch/DRIE-Pegasus/Pegasus-4| '''DRIE-Pegasus 4''']] | ||
|- | |- | ||
!style="background:silver; color:black;" align="center" valign="center" width=" | !style="background:silver; color:black;" align="center" valign="center" width="100" rowspan="2"|Purpose | ||
|style="background:Whitesmoke; color:black"| Primary | |style="background:Whitesmoke; color:black" width="80" | Primary | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
* Dry etching of 4" silicon | * Dry etching of 4" silicon | ||
| Line 63: | Line 75: | ||
* ? | * ? | ||
|style="background:LightGrey; color:black"| | |style="background:LightGrey; color:black"| | ||
* | * silicon | ||
|- | |- | ||
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Performance | !style="background:silver; color:black" align="center" valign="center" rowspan="2"|Performance | ||
| Line 75: | Line 87: | ||
* ? | * ? | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
* | * Depending on the recipe | ||
|- | |- | ||
|style="background:LightGrey; color:black"|Uniformity | |style="background:LightGrey; color:black"|Uniformity | ||
| Line 85: | Line 97: | ||
* ? | * ? | ||
|style="background:lightgrey; color:black"| | |style="background:lightgrey; color:black"| | ||
* | * Depending on the recipe | ||
|- | |- | ||
!style="background:silver; color:black" align="center" valign="center" rowspan="4"|Process parameter range | !style="background:silver; color:black" align="center" valign="center" rowspan="4"|Process parameter range | ||
| Line 109: | Line 121: | ||
* Ar: 0 to 283 sccm | * Ar: 0 to 283 sccm | ||
|style="background:lightgrey; color:black"| | |style="background:lightgrey; color:black"| | ||
* SF<sub>6</sub>: 0 to 1200 sccm | * SF<sub>6</sub>-1: 0 to 1200 sccm | ||
* SF<sub>6</sub>-2: 0 to 100 sccm | |||
* O<sub>2</sub>: 0 to 50 sccm | |||
* N<sub>2</sub>: 0 to 500 sccm | |||
* Ar: 0 to 283 sccm | |||
* He: 0 to 11 sccm | |||
|style="background:lightgrey; color:black"| | |||
* SF<sub>6</sub>-1: 0 to 1200 sccm | |||
* SF<sub>6</sub>-2: 0 to 100 sccm | |||
* O<sub>2</sub>: 0 to 200 sccm | * O<sub>2</sub>: 0 to 200 sccm | ||
* C<sub>4</sub>F<sub>8</sub>: 0 to 400 sccm | * C<sub>4</sub>F<sub>8</sub>: 0 to 400 sccm | ||
* Ar: 0 to 283 sccm | * Ar: 0 to 283 sccm | ||
|style="background:lightgrey; color:black"| | |style="background:lightgrey; color:black"| | ||
{| | {| | ||
*SF<sub>6</sub>: ?(<20) sccm | |||
*O<sub>2</sub>: 200 sccm | |||
*C<sub>4</sub>F<sub>8</sub>: 400 sccm | |||
*Ar: 283 sccm | |||
*He: 500 sccm | |||
*CF<sub>4</sub>: 100 sccm | |||
*H2: 100 sccm | |||
| | | | ||
| | | | ||
| Line 151: | Line 164: | ||
* Bosch processes with etch and dep cycles each split into three | * Bosch processes with etch and dep cycles each split into three | ||
* Parameter ramping during process steps | * Parameter ramping during process steps | ||
* SOI option to reduce notching at buried | * SOI option to reduce notching at buried oxide layers | ||
* Picoscope monitoring | * Picoscope monitoring | ||
* Claritas endpoint detection system | * Claritas endpoint detection system | ||
| Line 157: | Line 170: | ||
* Bosch processes with etch and dep cycles each split into three | * Bosch processes with etch and dep cycles each split into three | ||
* Parameter ramping during process steps | * Parameter ramping during process steps | ||
* SOI option to reduce notching at buried | * SOI option to reduce notching at buried oxide layers | ||
* Picoscope monitoring | * Picoscope monitoring | ||
* Verity OES | * Verity OES | ||
| Line 163: | Line 176: | ||
* Bosch processes with etch and dep cycles each split into three | * Bosch processes with etch and dep cycles each split into three | ||
* Parameter ramping during process steps | * Parameter ramping during process steps | ||
* Picoscope monitoring | |||
* SOI option to reduce notching at buried oxide layers | |||
|style="background:lightgrey; color:black"| | |style="background:lightgrey; color:black"| | ||
* Bosch processes with etch and dep cycles each split into three | * Bosch processes with etch and dep cycles each split into three | ||
* Parameter ramping during process steps | * Parameter ramping during process steps | ||
* Verity OES | |||
|- | |- | ||
!style="background:silver; color:black" align="center" valign="center" rowspan="4"|Substrates | !style="background:silver; color:black" align="center" valign="center" rowspan="4"|Substrates | ||
| Line 185: | Line 201: | ||
|style="background:lightgrey; color:black"| | |style="background:lightgrey; color:black"| | ||
* Load lock | * Load lock | ||
* MACS | * MACS (Multiplex Atmospheric Cassette System) | ||
|style="background:lightgrey; color:black"| | |style="background:lightgrey; color:black"| | ||
* Load lock | * Load lock | ||
|style="background:lightgrey; color:black" | |style="background:lightgrey; color:black" colspan="2"| | ||
* Vacuum cassette loader with two cassette stations and shared dealer chamber with Brooks robot | |||
* Vacuum cassette loader | |||
|- | |- | ||
| style="background:Whitesmoke; color:black"|Allowed materials | | style="background:Whitesmoke; color:black"|Allowed materials | ||
| Line 229: | Line 243: | ||
* zep resist | * zep resist | ||
* DUV stepper resist (barc + krf) | * DUV stepper resist (barc + krf) | ||
* Oxides and nitrides | * Silicon,Oxides and nitrides | ||
* Al, Cr masks | |||
|- | |- | ||
|} | |} | ||
| Line 235: | Line 250: | ||
== Process information == | == Process information == | ||
===Process notation=== | |||
Describing a process recipe on the Pegasus may sometimes be difficult because of the great flexibility of the instrument. A compact and precise notation is therefore required for the recipes. Click [[Specific_Process_Knowledge/Etch/DRIE-Pegasus/Notation|'''HERE''']] to find a short description | Describing a process recipe on the Pegasus may sometimes be difficult because of the great flexibility of the instrument. A compact and precise notation is therefore required for the recipes. Click [[Specific_Process_Knowledge/Etch/DRIE-Pegasus/Notation|'''HERE''']] to find a short description. | ||
A few hardware modifications have been made on the Pegasus since it was installed in 2010. The changes are listed in the table below under hardware options. | |||
===Hardware changes=== | |||
A few hardware modifications have been made on the Pegasus 1 since it was installed in 2010. The changes are listed in the table below under hardware options. | |||
| Line 250: | Line 270: | ||
! style="background:silver; color:black" | [[Specific Process Knowledge/Etch/DRIE-Pegasus/Pegasus-3| DRIE-Pegasus 3]] | ! style="background:silver; color:black" | [[Specific Process Knowledge/Etch/DRIE-Pegasus/Pegasus-3| DRIE-Pegasus 3]] | ||
! style="background:silver; color:black" | [[Specific Process Knowledge/Etch/DRIE-Pegasus/Pegasus-4| DRIE-Pegasus 4]] | ! style="background:silver; color:black" | [[Specific Process Knowledge/Etch/DRIE-Pegasus/Pegasus-4| DRIE-Pegasus 4]] | ||
|- valign="top" | |- valign="top" | ||
! style="background:lightgrey; color:black" | Manufactured | ! style="background:lightgrey; color:black" | Manufactured | ||
| style="background:lightgrey; color:black" | 2010 | | style="background:lightgrey; color:black" | 2010 | ||
| style="background:lightgrey; color:black" | 2010 | | style="background:lightgrey; color:black" | 2010 | ||
| style="background:lightgrey; color:black" | | | style="background:lightgrey; color:black" | 2010 | ||
| style="background:lightgrey; color:black" | | | style="background:lightgrey; color:black" | 2010 | ||
|- valign="top" | |- valign="top" | ||
! style="background:Whitesmoke; color:black" | Serial | ! style="background:Whitesmoke; color:black" | Serial | ||
| style="background:WhiteSmoke; color:black" | MP0636 | |||
| style="background:WhiteSmoke; color:black"| MP0641 | | style="background:WhiteSmoke; color:black"| MP0641 | ||
| style="background:WhiteSmoke; color:black"| CP0170 | | style="background:WhiteSmoke; color:black"| CP0170 | ||
| Line 282: | Line 296: | ||
| style="background:WhiteSmoke; color:black"| | | style="background:WhiteSmoke; color:black"| | ||
* [[Specific Process Knowledge/Etch/DRIE-Pegasus/showerheadchange|High flow plenum]] | * [[Specific Process Knowledge/Etch/DRIE-Pegasus/showerheadchange|High flow plenum]] | ||
| style="background:WhiteSmoke; color:black"| | * [[Specific Process Knowledge/Etch/DRIE-Pegasus/picoscope|Picoscope oscilloscope]] | ||
| style="background:WhiteSmoke; color:black"| | |||
* [[Specific Process Knowledge/Etch/DRIE-Pegasus/showerheadchange|High flow plenum]] | |||
* [[Specific Process Knowledge/Etch/DRIE-Pegasus/picoscope|Picoscope oscilloscope]] | |||
| style="background:WhiteSmoke; color:black"| ? | | style="background:WhiteSmoke; color:black"| ? | ||
|- | |- | ||
| Line 288: | Line 305: | ||
|} | |} | ||
= General Pegasus information = | |||
==Wafer bonding== | |||
To find information on how to bond wafers or chips to a carrier wafer, click [[Specific Process Knowledge/Etch/DryEtchProcessing/Bonding| '''HERE''']]. | |||
==Characterisation of etched trenches== | |||
The trenches in deep silicon trenches can be characterized in many ways. Being able to compare processes requires that a set of common measurements and calculations must be established. Click '''HERE''' to find more information about the parameters used on the DRIE-Pegasus process developme[[Specific Process Knowledge/Etch/DRIE-Pegasus/TrenchCharacterisation|nt]]. | |||
Latest revision as of 11:41, 21 October 2025
Feedback to this page: click here
The DRIE Pegasus tools at DTU Nanolab
Unless otherwise stated, all content on this page was created by Jonas Michael-Lindhard, DTU Nanolab
In 2010 DTU Nanolab acquired DRIE-Pegasus 1. As a state-of-the-art etch tool with excellent performance and great flexibility, it grew immensely popular and by 2015 it was apparent that we needed yet another tool to cope with the demand. Therefore, in 2016 Pegasus 2 was acquired from a closed-down lab and installed next to Pegasus 1.
Looking to expand our dry etching capabilities in 2017 we got an irresistible offer on a twin Pegasus system with cassette to cassette vacuum robot from a commercial fab. The twin Pegasus system (called Pegasus 3 and 4) is installed at the old cluster 2 location in cleanroom C1 and will run only 6" wafers. Pegasus 3 is the 6" silicon etch work horse and Pegasus 4 is converted (adding extra process gases) into a 6" dielectric etch tool that will supplement/replace the AOE.
This page was originally intended as a regular one-machine page (the Pegasus 1 page). However, as of 2018 with several tools, the page will serve as common page for all of our Pegasi with subpages for each tool.
The Bosch process
The DRIE Pegasus tools are state-of-art silicon dry etchers that offer outstanding performance in terms of etch rate, uniformity etc. They use the so-called Bosch process to achieve excellent control of the etched features. Click HERE to access the top of the page. The contents are:
- Description of the Bosch process
- Processing options on the Pegasus
- Modification of the showerhead
- RF matching
- Picoscope process monitoring
As of 2017, completing the Dry Etch TPT course is mandatory for all new users. On the TPT web page you will find a version of the latest lecture slides - here you will find information as well.
Links to the individual pages for the Pegasi
| Equipment | DRIE-Pegasus 1 | DRIE-Pegasus 2 | DRIE-Pegasus 3 | DRIE-Pegasus 4 | ||
|---|---|---|---|---|---|---|
| Purpose | Primary |
|
|
|
| |
| Alternative |
|
|
|
| ||
| Performance | Etch rates |
|
|
|
| |
| Uniformity |
|
|
|
| ||
| Process parameter range | RF powers |
|
|
|
| |
| Gas flows |
|
|
|
| ||
| Pressure and temperature |
|
|
|
| ||
| Process options |
|
|
|
| ||
| Substrates | Sizes |
|
|
|
| |
| Loading |
|
|
| |||
| Allowed materials |
|
|
|
| ||
| Possible masking materials |
|
|
|
| ||
Process information
Process notation
Describing a process recipe on the Pegasus may sometimes be difficult because of the great flexibility of the instrument. A compact and precise notation is therefore required for the recipes. Click HERE to find a short description.
Hardware changes
A few hardware modifications have been made on the Pegasus 1 since it was installed in 2010. The changes are listed in the table below under hardware options.
| DRIE-Pegasus 1 | DRIE-Pegasus 2 | DRIE-Pegasus 3 | DRIE-Pegasus 4 | |
|---|---|---|---|---|
| Manufactured | 2010 | 2010 | 2010 | 2010 |
| Serial | MP0636 | MP0641 | CP0170 | CP0171 |
| Electrode size | 4" | 6" | 6" | 6" |
| Hardware options | ? |
General Pegasus information
Wafer bonding
To find information on how to bond wafers or chips to a carrier wafer, click HERE.
Characterisation of etched trenches
The trenches in deep silicon trenches can be characterized in many ways. Being able to compare processes requires that a set of common measurements and calculations must be established. Click HERE to find more information about the parameters used on the DRIE-Pegasus process development.