Jump to content

Specific Process Knowledge/Etch/ICP Metal Etcher/silicon/nano/Sinan37: Difference between revisions

From LabAdviser
Jmli (talk | contribs)
No edit summary
Jmli (talk | contribs)
No edit summary
 
(3 intermediate revisions by the same user not shown)
Line 1: Line 1:
<!-- Ok, jmli 20170627 -->
<!-- Ok, jmli 20170627 -->
<!-- revised 1/6-2015 by jmli -->
<!-- revised 1/6-2015 by jmli -->
<!--Checked for updates on 10/7-2019 - ok/jmli -->
<!--Checked for updates on 24/8-2021. ok/ jmli-->
<!--Checked for updates on 4/4-2025 - ok/jmli -->
<!--Checked for updates on 4/4-2025 - ok/jmli -->
{| {{table}}
{| {{table}}
| align="center" style="background:#f0f0f0;"|'''Nominal trench line width'''
| align="center" style="background:#f0f0f0;"|'''Nominal trench line width'''

Latest revision as of 08:37, 4 April 2025


Nominal trench line width ' ' 30 60 90 120 150 Average Std. dev.
Etch rate nm/min 59 67 67 67 68 66 4
Sidewall angle degs 84 86 84 86 86 85 1
CD loss nm/edge -16 -31 -29 -36 -33 -29 8
CD loss foot nm/edge -16 -23 -14 -18 -12 -17 4
Bowing 7 23 15 10 9 13 7
Bottom curvature -27 -8 11 9 4 -2 15