Specific Process Knowledge/Thin film deposition/Deposition of Alumina: Difference between revisions
Appearance
No edit summary |
|||
| (13 intermediate revisions by 4 users not shown) | |||
| Line 1: | Line 1: | ||
'''Feedback to this page''': '''[mailto:labadviser@ | '''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Alumina click here]''' | ||
''All text by Nanolab staff'' | |||
==Deposition of | ==Deposition of Al<sub>2</sub>O<sub>3</sub>== | ||
Aluminium oxide (Alumina, Al<sub>2</sub>O<sub>3</sub> ) can be deposited by use of ALD (atomic layer deposition) or by | Aluminium oxide (Alumina, Al<sub>2</sub>O<sub>3</sub>) can be deposited by use of ALD (atomic layer deposition), by e-beam evaporation or by sputtering. During the evaporation or sputter deposition oxygen is added to the chamber resulting in aluminium oxide on the sample. | ||
*[[Specific_Process_Knowledge/Thin_film_deposition/ALD_Picosun_R200/Al2O3_deposition_using_ALD|Al<sub>2</sub>O<sub>3</sub> deposition using ALD]] | *[[Specific_Process_Knowledge/Thin_film_deposition/ALD_Picosun_R200/Al2O3_deposition_using_ALD|Al<sub>2</sub>O<sub>3</sub> deposition using ALD]] | ||
*[[Specific Process Knowledge/Thin film deposition/Lesker|Lesker Sputter System]] | *[[Specific Process Knowledge/Thin film deposition/Lesker|Sputter-System(Lesker)]] | ||
*[[Specific_Process_Knowledge/Thin_film_deposition/Cluster-based_multi-chamber_high_vacuum_sputtering_deposition_system#Standard_recipe_performance|Sputter-System Metal-Oxide(PC1)]] | |||
*[[Specific_Process_Knowledge/Thin_film_deposition/Deposition of Alumina/E-beam Evaporation of Al2O3 in Temescal-2|Evaporation of Al<sub>2</sub>O<sub>3</sub> in E-Beam Evaporator (10-pockets)]] | |||
==Comparison of the methods for deposition of Alumium Oxide== | ==Comparison of the methods for deposition of Alumium Oxide== | ||
| Line 16: | Line 19: | ||
|-style="background:silver; color:black" | |-style="background:silver; color:black" | ||
! | ! | ||
![[Specific Process Knowledge/Thin film deposition/Lesker|Sputter System Lesker]] | ![[Specific Process Knowledge/Thin film deposition/Lesker|Sputter-System(Lesker)]] | ||
![[ | ![[Specific_Process_Knowledge/Thin_film_deposition/Cluster-based_multi-chamber_high_vacuum_sputtering_deposition_system|Sputter-System Metal-Oxide(PC1)]] | ||
![[Specific Process Knowledge/Thin film deposition/ALD Picosun R200|ALD Picosun 200]] | ![[Specific Process Knowledge/Thin film deposition/ALD Picosun R200|ALD Picosun 200]] | ||
![[Specific Process Knowledge/Thin film deposition/10-pocket e-beam evaporator|10-pocket e-beam evaporator]] | |||
|- | |- | ||
| Line 26: | Line 30: | ||
| | | | ||
*RF sputtering from Al<sub>2</sub>O<sub>3</sub> target | *RF sputtering from Al<sub>2</sub>O<sub>3</sub> target | ||
*Reactive | *Reactive sputtering | ||
| | | | ||
*Reactive | *RF sputtering from Al<sub>2</sub>O<sub>3</sub> target | ||
*Pulsed DC reactive sputtering | |||
*Reactive HIPIMS (high-power impulse magnetron sputtering) | |||
| | | | ||
*ALD (atomic layer deposition) of Al<sub>2</sub>O<sub>3</sub> | *ALD (atomic layer deposition) of Al<sub>2</sub>O<sub>3</sub> | ||
| | |||
*E-beam evaporation of Al<sub>2</sub>O<sub>3</sub> pellets or of Al in an O<sub>2</sub> flow | |||
|- | |- | ||
| Line 42: | Line 50: | ||
| | | | ||
*Al<sub>2</sub>O<sub>3</sub>, very good | *Al<sub>2</sub>O<sub>3</sub>, very good | ||
| | |||
*Not tested yet | |||
|- | |- | ||
| Line 48: | Line 58: | ||
!Film Thickness | !Film Thickness | ||
| | | | ||
* | *few nm - 200 nm | ||
| | | | ||
* | *few nm - 200-300 nm | ||
| | | | ||
* 0nm - | * 0nm - 100 nm | ||
| | |||
*few nm - 200 nm (talk to staff if you wish to deposit more than 100 nm as it can cause flaking in the chamber) | |||
|- | |- | ||
| Line 58: | Line 70: | ||
!Deposition rate | !Deposition rate | ||
| | | | ||
* 0 | * 0.3 nm/min | ||
| | | | ||
* | * About 1.7 nm/min, depends on sputtering parameters | ||
| | | | ||
*0. | *0.088 - 0.097 nm/cycle (Using the "Al2O3" recipe, temperature dependent) | ||
| | |||
* 1-2 Å/s | |||
|- | |- | ||
| Line 72: | Line 85: | ||
*unknown | *unknown | ||
| | | | ||
* | *unknown | ||
| | | | ||
*Very good. Covers sample everywhere (but long purge time needed for very high aspect ratio structures) | *Very good. Covers sample everywhere (but long purge time needed for very high aspect ratio structures) | ||
| | |||
* We expect no step coverage unless using tilt holder, in which case the step coverage can be very good and can be tuned. | |||
|- | |- | ||
| Line 80: | Line 95: | ||
!Process Temperature | !Process Temperature | ||
| | | | ||
* Up to | * room temperature | ||
| | |||
* Up to 600 °C | |||
| | | | ||
* | *150 °C - 350 °C | ||
| | | | ||
* | * Up to 250 °C | ||
|- | |- | ||
| Line 92: | Line 109: | ||
| | | | ||
| | | | ||
* - | *See [[Specific_Process_Knowledge/Thin_film_deposition/Cluster-based_multi-chamber_high_vacuum_sputtering_deposition_system#Standard_recipe_performance|deposition conditions]] | ||
| | | | ||
*[[Specific Process Knowledge/Thin film deposition/ALD Picosun R200/Al2O3 deposition using ALD|Al<sub>2</sub>O<sub>3</sub> deposition using ALD]] | *[[Specific Process Knowledge/Thin film deposition/ALD Picosun R200/Al2O3 deposition using ALD|Al<sub>2</sub>O<sub>3</sub> deposition using ALD]] | ||
| | |||
|- | |- | ||
| Line 105: | Line 124: | ||
* 1x 150 mm wafer | * 1x 150 mm wafer | ||
| | | | ||
* 100 mm | * chips | ||
* 150 mm | * 10x 100 mm wafer | ||
* 10x 150 mm wafer | |||
| | | | ||
*1-5 100 mm wafers | *1-5 100 mm wafers | ||
*1-5 150 mm wafers | *1-5 150 mm wafers | ||
*1-3 200 mm wafers | |||
*Several smaller samples | *Several smaller samples | ||
| | |||
* chips | |||
* 1-3 x 100 mm wafers | |||
* 1-3 x 150 mm wafers | |||
* 1-3 x 200 mm wafers | |||
|- | |- | ||
| Line 117: | Line 143: | ||
!'''Allowed materials''' | !'''Allowed materials''' | ||
| | | | ||
*almost any | *almost any that does not degas | ||
| | | | ||
* | *almost any that does not degas. Note special carrier for III-V materials. See [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=441 cross-contamination sheet]. | ||
| | | | ||
*Silicon | *Silicon | ||
| Line 136: | Line 155: | ||
*III-V materials (use dedicated carrier wafer) | *III-V materials (use dedicated carrier wafer) | ||
*Polymers (depending on the melting point/deposition temperature, use carrier wafer) | *Polymers (depending on the melting point/deposition temperature, use carrier wafer) | ||
| | |||
*almost any that does not degas. See [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=511 cross-contamination sheet] | |||
|- | |- | ||
|} | |} | ||