Specific Process Knowledge/Etch/III-V ICP/GaAsnano: Difference between revisions

From LabAdviser
Jmli (talk | contribs)
No edit summary
Bghe (talk | contribs)
No edit summary
 
(2 intermediate revisions by 2 users not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Etch/III-V_ICP/GaAsnano click here]'''  
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/III-V_ICP/GaAsnano click here]'''  
<!--Checked for updates on 18/8-2021 - ok/bghe -->
=== GaAs nano etch ===
=== GaAs nano etch ===


Line 29: Line 29:


{| border="1" cellspacing="2" cellpadding="3"  align="left"
{| border="1" cellspacing="2" cellpadding="3"  align="left"
|colspan="2" align="center"| '''Results (GaAs Nano Etch)'''  
|colspan="2" align="center"| '''Results (GaAs Nano Etch)''' ''from 2011 by Thor Ansbæk @photonic''
|-  
|-  
|GaAs
|GaAs

Latest revision as of 14:42, 18 August 2021

Feedback to this page: click here

GaAs nano etch

Recipe GaAs Nano Etch
Cl2 flow 4 sccm
Ar flow 12 sccm
Platen power 80 W
Coil power 700 W
Pressure 6 mTorr
Platen chiller temperature 20 oC


Results (GaAs Nano Etch) from 2011 by Thor Ansbæk @photonic
GaAs 5 nm/s
AlInP 1 nm/s
HSQ 1.5 nm/s
ZEP520a 2 nm/s
Si3N4 2 nm/s
GaAs sample with a ZEP520a masking layer etched for 1 min 15 s with the "GaAs Nano Etch" recipe. Thor Ansbæk, DTU Photonics, 2011.