Line 1: Line 1:
 
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/DRIE-Pegasus/Isotropic click here]'''
<!--Checked for updates on 2/10-2020 - ok/jmli -->
<!--Checked for updates on 14/5-2018 - ok/jmli -->
<!--Checked for updates on 4/9-2025 - ok/jmli -->


{| border="1" cellpadding="1" cellspacing="0" style="text-align:center;"
{| border="1" cellpadding="1" cellspacing="0" style="text-align:center;"
Line 17: Line 20:
! width="100" | Key words
! width="100" | Key words
|-
|-
! mediumiso1   <!-- recipe name -->
! Mediumiso1   <!-- recipe name -->
| -        <!-- step -->
| -        <!-- step -->
| 20      <!-- chiller temp -->
| 20      <!-- chiller temp -->
Line 28: Line 31:
| 3      <!-- platen power -->
| 3      <!-- platen power -->
|[[Specific Process Knowledge/Etch/DRIE-Pegasus/Isotropic/mediumiso1|1]]    <!-- link processes -->
|[[Specific Process Knowledge/Etch/DRIE-Pegasus/Isotropic/mediumiso1|1]]    <!-- link processes -->
| NA     <!-- keywords -->
| Works great. Used extensively for Ph.D. thesis of Peter Emil Larsen     <!-- keywords -->
|-
|-
! Isoslow7      <!-- recipe name -->
! Isoslow7      <!-- recipe name -->
|       <!-- step -->
| -      <!-- step -->
| 10        <!-- chiller temp -->
| 10        <!-- chiller temp -->
| 10      <!-- pressure -->
| 10      <!-- pressure -->
|       <!-- C4F8 flow -->
| 0      <!-- C4F8 flow -->
| 80      <!-- SF6 flow -->
| 80      <!-- SF6 flow -->
|       <!-- O2 flow -->
| 0      <!-- O2 flow -->
| 0      <!-- Ar flow -->
| 150      <!-- coil power -->
| 150      <!-- coil power -->
| 3      <!-- platen power -->
| 3      <!-- platen power -->
Line 49: Line 53:
|        <!-- SF6 flow -->
|        <!-- SF6 flow -->
|        <!-- O2 flow -->
|        <!-- O2 flow -->
|      <!-- Ar flow -->
|        <!-- coil power -->
|        <!-- coil power -->
|        <!-- platen power -->
|        <!-- platen power -->

Latest revision as of 10:40, 4 September 2025

Feedback to this page: click here

Mediumiso
Recipe Step Temperature Pressure C4F8 SF6 O2 Ar Coil Platen Runs Key words
Mediumiso1 - 20 25 0 150 0 0 600 3 1 Works great. Used extensively for Ph.D. thesis of Peter Emil Larsen
Isoslow7 - 10 10 0 80 0 0 150 3 1
-