Specific Process Knowledge/Etch/DRIE-Pegasus/ProcessA/PrA-1: Difference between revisions
Appearance
No edit summary |
No edit summary |
||
| (5 intermediate revisions by the same user not shown) | |||
| Line 1: | Line 1: | ||
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/DRIE-Pegasus/ProcessA/PrA-1 click here]''' | |||
<!--Checked for updates on 30/7-2018 - ok/jmli --> | |||
<!--Checked for updates on 5/10-2020 - ok/jmli --> | |||
<!--Checked for updates on 28/6-2023 - ok/jmli --> | |||
<!--Checked for updates on 4/9-2025 - ok/jmli --> | |||
{{contentbydryetch}} | |||
{| border="2" cellpadding="0" cellspacing="0" style="text-align:center;" | {| border="2" cellpadding="0" cellspacing="0" style="text-align:center;" | ||
| Line 74: | Line 80: | ||
| C04047.02 | | C04047.02 | ||
| | | | ||
[[file:C04047.02 086.jpg|150px|frameless ]] | |||
[[file:C04047.02 087.jpg|150px|frameless ]] | |||
[[file:C04047.02 088.jpg|150px|frameless ]] | |||
[[file:C04047.02 089.jpg|150px|frameless ]] | |||
[[file:C04047.02 090.jpg|150px|frameless ]] | |||
[[file:C04047.02 091.jpg|150px|frameless ]] | |||
[[file:C04047.02 092.jpg|150px|frameless ]] | |||
[[file:C04047.02 093.jpg|150px|frameless ]] | |||
[[file:C04047.02 094.jpg|150px|frameless ]] | |||
[[file:C04047.02 095.jpg|150px|frameless ]] | |||
[[file:C04047.02 096.jpg|150px|frameless ]] | |||
[[file:C04047.02 083.jpg|150px|frameless ]] | |||
[[file:C04047.02 084.jpg|150px|frameless ]] | |||
[[file:C04047.02 085.jpg|150px|frameless ]] | |||
|- | |- | ||
| 3/6-2016 | | 3/6-2016 | ||
| Line 83: | Line 102: | ||
| C04047.05 | | C04047.05 | ||
| | | | ||
[[file:C04047.05 132.jpg|150px|frameless ]] | |||
[[file:C04047.05 133.jpg|150px|frameless ]] | |||
[[file:C04047.05 134.jpg|150px|frameless ]] | |||
[[file:C04047.05 135.jpg|150px|frameless ]] | |||
[[file:C04047.05 136.jpg|150px|frameless ]] | |||
[[file:C04047.05 137.jpg|150px|frameless ]] | |||
[[file:C04047.05 138.jpg|150px|frameless ]] | |||
[[file:C04047.05 124.jpg|150px|frameless ]] | |||
[[file:C04047.05 125.jpg|150px|frameless ]] | |||
[[file:C04047.05 126.jpg|150px|frameless ]] | |||
[[file:C04047.05 127.jpg|150px|frameless ]] | |||
[[file:C04047.05 128.jpg|150px|frameless ]] | |||
[[file:C04047.05 129.jpg|150px|frameless ]] | |||
[[file:C04047.05 130.jpg|150px|frameless ]] | |||
[[file:C04047.05 131.jpg|150px|frameless ]] | |||
|- | |- | ||
|} | |} | ||
Latest revision as of 11:59, 4 September 2025
Feedback to this page: click here
Unless otherwise stated, the content of this page was created by the dry etch group at DTU Nanolab
| Date | Substrate Information | Process Information | SEM Images | |||
|---|---|---|---|---|---|---|
| Wafer info | Exposed area | Conditioning | Recipe | Wafer ID | ||
| 2/5-2016 | 4" Travka20 Wafer | 20 % Si | 3 minute TDESC clean | PrA-1, 80 cycles or 14:40 minutes | C03991.02 |
|
| 2/5-2016 | 4" Travka20 Wafer | 20 % Si | 3 minute TDESC clean | PrA-1, 80 cycles or 14:40 minutes | C03991.05 | |
| 3/6-2016 | 4" Travka20 Wafer | 20 % Si | 3 minute TDESC clean | PrA-1, 80 cycles or 14:40 minutes | C04047.02 | |
| 3/6-2016 | 4" Travka20 Wafer | 20 % Si | 3 minute TDESC clean | PrA-1, 80 cycles or 14:40 minutes | C04047.05 | |